Lampiran A.47 No. Dokumen WB-MC2-ENG-IK47 Tanggal Berlaku PENGUJIAN IGNITION LOSS SEMEN DAN FLY ASH 12/03/2019 INSTRUKSI KERJA

Judul : PT WIJAYA KARYA BETON Tbk

No. Revisi Halaman 00 12 dari 74 Tanggal Review 12/03/2022

A. Referensi 1. GB/T 176 -2017, Methods for chemical analysis of cement B. Bahan 1. Semen 2. Fly Ash C. Alat 1. 2. 3. 4.

Timbangan 100g, akurat 0,0001 Oven suhu tinggi (950±25)˚C Cawan Desikator

D. Urutan Kerja 1 Timbang sampel seberat 1g akurat hingga 0,0001 g (m). 2 Timbang berat cawan kosong 3 Letakkan sampel ke dalam cawan kemudian di oven pada suhu (950Β±25)oC selama 15 – 20 menit 4 Angkat dan dinginkan dalam desikator lalu timbang (m1) E. Perhitungan

Keterangan : WLOI = Persentase Ignition Loss (%) m = Berat sampel awal (g) m1 = Berat sampel setelah dioven (g) F. Rekaman 1. Laporan Cement Test Record (Form : WB-MC2-ENG-F19, F20 dan F21) 2. Laporan Fly Ash Test Record (Form : WB-MC2-ENG-F15 & 16)

Scan disini

Untuk menonton video

Keterangan: *referensi merujuk pada prosedur WB-ENG-PS-06 Form : WB-QMS-PS-01-F07

Rev : 00


Turn static files into dynamic content formats.

CreateΒ aΒ flipbook

Articles inside

A.12 Bulk Density and Void Ratio WB-HSR-PS-01-IK12 00

1min
page 49

Pengujian Sulfate Content WB-HSR-PS-12-IK5 00

1min
page 72

Pengujian Insoluble Content WB-HSR-PS-12-IK2 00

1min
page 68

A.11 Apparent Density WB-HSR-PS-01-IK11 00

1min
page 48

A.7 Organic Content WB-HSR-PS-01-IK7 00

1min
page 44

A.6 Compressive Strength WB-HSR-PS-01-IK6 00

1min
page 43

A.8 Elongation and Flakyness WB-HSR-PS-01-IK8 00

2min
page 45

A.10 Kadar Sulfida dan Sulfat WB-HSR-PS-01-IK10 00

1min
page 47

A.5 Water Absorbtion WB-HSR-PS-01-IK5 00

1min
page 42

A.27 Moisture Content WB-HSR-PS-06-IK27 00

1min
page 32

Kadar Sulfida dan Sulfat WB-HSR-PS-06-IK32 00

1min
page 37

A.2 Sieve Analysis WB-HSR-PS-01-IK2 00

1min
page 39

A.31 Kloride Content WB-HSR-PS-06-IK31 00

1min
page 36

A.14 Water Content WB-HSR-PS-05-IK12 00

1min
page 21

A.25 Solidness WB-HSR-PS-06-IK25 00

1min
page 30

A.11 Alkali Content WB-HSR-PS-05-IK11 00

1min
page 17

A.26 Lightweight Content WB-HSR-PS-06-IK26 00

1min
page 31

A.22 Clay Lump Content WB-HSR-PS-06-IK22 00

1min
page 27

A.21 Silt Content WB-HSR-PS-06-IK21 00

1min
page 26

A.16 CaO Content WB-HSR-PS-05-IK12 00

3min
pages 23-24

A.10 Free CaO Content WB-HSR-PS-05-IK10 00

1min
page 16

A.7 Ignition Loss WB-HSR-PS-05-IK7 00

1min
page 13

A.4 Stabilitas Semen WB-HSR-PS-05-IK4 00

1min
page 10

A.8 MgO Content WB-HSR-PS-05-IK8 00

1min
page 14

A.9 SO 3 Content WB-HSR-PS-05-IK9 00

1min
page 15

A.3 Specific Surface Area WB-HSR-PS-05-IK3 00

1min
page 9

A.6 Flexural Strength WB-HSR-PS-05-IK6 00

1min
page 12

A.2 WB-HSR-PS-05-IK2 00

1min
page 8

A.5 Compressive Strength WB-HSR-PS-05-IK5 00

1min
page 11
Issuu converts static files into: digital portfolios, online yearbooks, online catalogs, digital photo albums and more. Sign up and create your flipbook.
E-Book QCI Pasundan MC2 by Unit Mobile Concrete 2 PT Wijaya Karya Beton - Issuu