Volume XXXVI - Issue II - June.,2026
Prof. Ailton de Souza Gomez Emeritus Professor, IMA/UFRJ
021 Pol, 2 B C 16 Preto Ouro th
Some types of fiber chemical treatment
Pêndulo para Impacto CHARPY/IZOD para Polímeros - Modelos IT504/IT503 • • • • • • • • • • •
Figura 1 – modelo IT504
Construção robusta; Pêndulo aerodinâmico que pode acomodar massas para aumentar a capacidade do equipamento; Unidades de energia selecionáveis: J, kgf.m, kgf.cm, in.Ibf e ft.Ibf; Outras unidades selecionáveis: J/m, kgf.m/m, in.lbf/in ou ft.lbf/in - kJ/m², kgf.m/m², in.lbf/in² ou ft.lbf/in²; Simples e rápida substituição entre os acessórios CHARPY/IZOD; Opção de inserção do tipo de quebra da amostra; Correção automática ou manual de "TOSS"; Auto calibração do pêndulo; Inserção automática ou manual da identificação da amostra; Atende às normas: ASTM D256 e ISO 180 (IZOD), ASTM D6110 e Figura 2 – modelo IT503 ISO 179 (CHARPY), entre outras.
OPCIONAIS DO MODELO IT504 • • •
Martelos opcionais de 1J IZOD ISO 180 – 0,5/1J CHARPY ISO 179 e 25/50J CHARPY; Câmara para ensaios a baixa temperatura (-60°C); Software.
Além das características do modelo IT504, o modelo IT503 possui as seguintes características: • Portas de segurança que garantem que o pêndulo seja liberado apenas após travamento das portas; • Atende a todas as diretivas Europeias de Segurança (CE);
Medidor de índice de fluidez (plastômetro de extrusão) modelos MP1200/MP1200M • • • • • • • • •
Tela de 7,1” sensível ao toque (touch screen) e de fácil programação pelo usuário; Parâmetros de teste podem ser armazenados ou digitados a cada novo teste; Controle de temperatura através de três zonas de aquecimento; Retirada da matriz pela parte inferior do forno; Conectividade USB; Alarmes sonoros para término de pré-aquecimento e tempo de corte; Operação até 450°c, com resolução de 0,1°c; Porta USB para comunicação com impressora ou computador (opcionais); Atende às normas ASTM D1238 e D3364, ISO 1133-1 e ISO 1133-2, BS 2782, DIN 53735, JIS K7210.
OPCIONAIS DOS MODELOS MP1200/MP1200M •
Figura 1 – modelo MP1200
• • •
Transdutor programável de deslocamento do pistão para método b (MVR); Corte automático; Sistema de seleção das massas (mp1200m); Software;
DINATESTE IND E COM LTDA
SÃO PAULO - SP Representante exclusiva no Brasil da marca Tinius Olsen www.dinateste.com.br dinateste@dinateste.com.br Tel: (11) 3723-2710
Figura 2 – modelo MP1200M (MOTORIZADO)
ISSN 0104-1428 (printed) ISSN 1678-5169 (online)
P o l í m e r o s - I ss u e I I - V o l u m e X X X V I - 2 0 2 6 I n d e x e d i n : “ C h e m ic a l A b s t r a c t s ” — “ RA P RA A b s t r a c t s ” — “ A l l - R u s s i a n I n s t i t u t e o f S ci e n c e a n d T e c h n ic a l I n f o r m a t i o n ” — “ L a t i n d e x ” — “ W e b o f S ci e n c e ”
Polímeros E d i t o r i a l C o u nci l
Editorial Committee
Edvani Curti Muniz (UFPI/DQUI; UEM/DQI)- President
Sebastião V. Canevarolo Jr. – Editor-in-Chief
Members
A ss o ci a t e E d i t o r s
Alain Dufresne (Grenoble INP/Pagora) Ana V. A. Machado Nóbrega (UMinho/DEP) Antonio Aprigio S. Curvelo (USP/IQSC) Artur José Monteiro Valente (UC/DQ) Bluma G. Soares (UFRJ/IMA) César Liberato Petzhold (UFRGS/IQ) Cristina T. Andrade (UFRJ/IQ) Daniela Becker (UDESC/DEM) Denise F. S. Petri (USP/IQ) Edson R. Simielli (Simielli - Soluções em Polímeros) Elias Hage Jr. (Retired – UFSCar/DEMa) Janaina S. Crespo (UCS/DEFQ) José Alexandrino de Sousa (Retired – UFSCar/DEMa) José António C. Gomes Covas (UMinho/IPC) José Carlos C. S. Pinto (UFRJ/COPPE) Júlio Harada (Harada Hajime Machado Consutoria Ltda) Luiz Antonio Pessan (UFSCar/DEMa) Luiz Henrique C. Mattoso (EMBRAPA) Marco Aurelio De Paoli (UNICAMP/IQ) María del Mar Orta Cuevas (US/QA) Nikos Hadjikristidis (KAUST/ PSE) Paula Moldenaers (KU Leuven/CIT) Roberto Pantani, (UNISA/DIIn) Rodrigo Lambert Oréfice (UFMG/DEMET) Sandra A. Cruz (UFSCar/DQ) Sebastião V. Canevarolo Jr. (Retired – UFSCar/DEMa) Silvio Manrich (Retired – UFSCar/DEMa) You-Lo Hsieh (UC Davis/BAE)
Alain Dufresne Artur José Monteiro Valente Bluma G. Soares César Liberato Petzhold José António C. Gomes Covas José Carlos C. S. Pinto Paula Moldenaers Roberto Pantani Rodrigo Lambert Oréfice
In memoriam Aliton S. Gomes (UFRJ/IMA) Richard G. Weiss (Georgetown University/Chemistry)
D e s k t o p P u b l is h in g
www.editoracubo.com.br
“Polímeros” is a publication of the Associação Brasileira de Polímeros São Paulo 994 St. São Carlos, SP, Brazil, 13560-053 Phone: +55 16 3374-3949 emails: abpol@abpol.org.br / revista@abpol.org.br http://www.abpol.org.br Date of publication: June 2026
Financial support:
Available online at: www.scielo.br
Polímeros / Associação Brasileira de Polímeros. vol. 1, nº 1 (1991) -.São Carlos: ABPol, 1991Quarterly v. 36, nº 2 (June 2026) ISSN 0104-1428 ISSN 1678-5169 (electronic version)
Website of the “Polímeros”: www.revistapolimeros.org.br
1. Polímeros. l. Associação Brasileira de Polímeros. Polímeros, 36(2), 2026
E1
E E E E E E E E E E E E E E E E E E E E E E E E E E E E
I
Editorial Section Editorial................................................................................................................................................................................................E3 News....................................................................................................................................................................................................E5 Agenda.................................................................................................................................................................................................E6 Funding Institutions.............................................................................................................................................................................E7
R e vi e w A r t ic l e
N
Recent advances in natural fiber treatments for enhanced composite performance
Mehmet Cihan, Marcos Antonio Gimenes Benega and Hélio Ribeiro ............................................................................................ e20260016
Application of biopolymers in hydrogels for tissue repair with bioextracts: systematic review
Otávio Soares Nascimento, Adriano Freitas de Santana, Cláudia Sampaio de Andrade Lima, Ana Cristina Silveira Martins and Ricardo Yara .................................................................................................................................................................................... e20260019
O r i g in a l A r t ic l e
D
Thermal and spectroscopic study of irradiated polymeric systems
Rochele Klering, Thaíses Lima, Patricia Araújo, Renata Santos, Katia Aquino and Elmo Araújo ................................................ e20260013
From filaments to membranes: additive manufacturing of Ecovio® for oil–water separation
Iago Rodrigues de Abreu, Fábio Delano Penha Marques Torres, Arthur Antônio Sousa Sampaio, Rudy Folkersma, Laura Hecker de Carvalho, Lucas Rafael Carneiro da Silva, Tatianny Soares Alves and Renata Barbosa ................................... e20260014
Optimization of pultruded hybrid bio-filled glass fiber-reinforced composites for lightweight forearm application
E
Rajesh Kumar Chandel, Rahul Vaishya, Anish Kumar Bisht, Anurag Gupta, Manoj Kumar Singh and Suchart Siengchin .......... e20260015
Research on anti-graffiti coating of nanosilica-modified two-component waterborne polyurethane
Qin Li, Dingding Xiang, Lei Shi, Qian Zeng, Rui Han and Wenhai Lin .......................................................................................... e20260018
Surface-modified Agave vilmoriniana fibers for enhanced thermo-mechanical and interfacial performance in composites
Gowtham Saravanan and Ramakrishnan Thirumalaisamy ............................................................................................................. e20260020
Innovations in sustainable additive manufacturing: PLA, Amazon wood waste, Brazil nut oil
Jackeline Lira Bremgartner, Joaquim dos Santos, Lizandro Manzato Vitor Bremgartner and Claudete Catanhede do Nascimento ....... e20260022
X
Sorption of phenanthrene by crosslinked polymers with varied monomeric compositions
Rafael de Lima Pinto, Ezaine Cristina Corrêa Torquato, Luciana da Cunha Costa, Caroline Felix Carvalho and Mônica Regina da Costa Marques Calderari .................................................................................................................................. e20260021
Polylactic acid with oat oil: a biodegradable material intended for food packaging
Lucas Nunes Fonseca Boechat, Rodrigo Gomes de Amorim, Fábio Silveira Reis, Marianna de Oliveira da Costa Maia Pinto, Everton Rangel Bispo, Antonieta Middea, Edla Maria Bezerra Lima, Antonio Renato Bigansolli, Danieli Martins do Carmo, Belmira Benedita Lima-Kühn, Cristiane Hess de Azevedo Meleiro, Rosane Nora Castro and Renata Nunes Oliveira ................. e20260023
Ferula biomass: characterization and biosorption studies for the removal of dyes
Moubarek Mébarki, Hassiba Bokhari, Yasmina Benabdesslem, Ahmed Khelifaoui & Kadda Hachem.......................................... e20260024
S h o r t C o m m u nic a t i o n Development of a glycerol–CuSO4 polymer for high gamma ionizing radiation dosimetry
Gabriela Pontes Cardoso, Jony Marques Geraldo and Adriana de Souza Medeiros Batista ......................................................... e20260017
E2
Polímeros, 36(2), 2026
ISSN 1678-5169 (Online)
Polímeros: Ciência e Tecnologia with higher Impact Factor welcomes New Editorial Board Members Edvani Curti Muniz1,2*
D I
President of the Editorial Board of Polímeros: Ciência e Tecnologia, Departamento de Química, Universidade Federal do Piauí, 64049-550, Teresina, PI, Brasil 1
2
E
* munizec@ufpi.edu.br
T
Dear readers, authors, reviewers and contributors. The new 2026 edition of the Journal of Citation Reports (JCR) has been published, and our journal’s new impact factor is 1.6, an increase considering the last two editions (2024 was 1.000 – 60%; and 2025 was 1.4 – 14.3%). The continued growth of Polímeros is both encouraging and highly significant, reflecting the journal’s increasing recognition within the scientific community. Sustaining this progress, however, requires the ongoing dedication and collective efforts of the Editorial Committee and the Editorial Board. Likewise, the continued success of Polímeros depends on the active engagement of authors through the submission of high-quality manuscripts and on the invaluable contribution of reviewers, whose careful and rigorous evaluations ensure the scientific excellence of the published work. The steady increase in citations received by articles published in Polímeros further demonstrates the journal’s growing visibility, impact, and consolidation as a respected reference in the field of polymer science. We express our sincere gratitude to the members of the Editorial Committee and the Editorial Board, the funding agencies, the authors, and the reviewers for their dedication and commitment. We also acknowledge the indispensable support provided by the ABPol Secretariat, whose continuous assistance plays a fundamental role in the successful operation and ongoing development of Polímeros. I would like to take this opportunity to warmly welcome the following distinguished researchers, recently appointed as new members of the Polímeros Editorial Board, who will undoubtedly enrich and expand the journal’s expertise. The journal Polímeros: Ciência e Tecnologia has been making efforts to achieve gender balance in its editorial board:
O
• Ana Vera Alves Machado Nóbrega – University of Minho, Portugal • You-Lo Hsieh – University of California, Davis, United States • Maria del Mar Orta Cuervas – Universidad de Sevilla, Spain • Denise Freitas Siqueira Petri – University of São Paulo (USP), Brazil • Daniela Becker – State University of Santa Catarina, Brazil • Janaína da Silva Crespo – University of Caxias do Sul (UCS), Brazil • Sandra Andrea Cruz – Federal University of São Carlos (UFSCar), Brazil Their outstanding academic contributions, scientific leadership, and expertise in the field of polymer science and technology will greatly strengthen our journal’s mission of promoting excellence, innovation, and international collaboration in scientific publishing. We are delighted to have them join the Editorial Board and look forward to their valuable contributions to the continued growth and impact of Polímeros: Ciência e Tecnologia. So, the expectative is that the next FI increase still more, for consolidating the Polímeros. Prof. Dr. Edvani Curti Muniz President of the Editorial Board of Polímeros: Ciência e Tecnologia
Polímeros, 36(2), 2 026
E3
R I A L
Referência em Metrologia Científica e Analítica Para Laboratórios, Controle de Qualidade, Desenvolvimento e Pesquisa incluindo Nanotecnologia. Conectando inovação, tecnologia e conhecimento no universo dos polímeros
Espectrofotômetro Colorimétrico, TR520
Moinho para preparação de amostra, Pulverisette14
Peneirador a Vácuo, e200 LS Analisador de Tamanho e Distribuição de Particulas, MS3000+
altmann.com.br
POLYMERS THAT CRAWL LIKE WORMS: HOW MATERIALS CAN DEVELOP DIRECTION WITHOUT BEING TOLD WHERE TO GO New findings can help to better understand DNA dynamics in living cells Researchers at the University of Vienna have uncovered a surprising phenomenon: polymer chains with segments that simply fluctuate at different intensities can spontaneously develop directional, persistent motion when densely packed – even though nothing in the system points them in any particular direction. This “entropic tug of war,” driven by fundamental physical constraints, could help explain how DNA organizes and moves inside living cells, and may lead to new materials. The study was currently published in Physical Review X. “Think of a chain threaded through a dense forest of trees, which represent obstacles posed by the other chains in the system. One end of the chain is being shaken much more vigorously than the other,” explains lead author Jan Smrek from the Faculty of Physics at the University of Vienna. “You might expect it to just wiggle randomly in place. But we found that because the chain has to find its way by going in-between the trees, the difference in shaking intensity creates an imbalance that actually propels the entire chain forward through the forest.” This refers to a polymer, a large molecule consisting of many units linked together in a long chain, such as DNA. The Viennese research team – Adam Höfler, Iurii Chubak, Christos Likos and Jan Smrek – used computer simulations and analytical theory to show that this directed motion arises purely from topological constraints. When polymer chains are entangled and cannot pass through each other, segments with stronger fluctuations generate larger entropic forces. This creates an imbalance that pushes the entire chain forward along its own contour, with the stronger fluctuating part acting as the “head of the snake” moving through the forest of obstacles. Unlike previous active polymer models that build upon directional forces, this mechanism requires only a difference in fluctuation magnitude between segments. The finding has direct relevance to chromatin – the complex of DNA and proteins in cell nuclei. Various cellular processes like transcription and DNA repair create localized regions of enhanced activity along the chromatin fiber. The researchers’ work suggests these activity differences alone could drive the coherent chromatin motions observed in living cells. The study also reveals how the dynamics depend on the degree of chain entanglement. At higher densities, the directed motion becomes faster and more pronounced. The researchers found that individual segments can exhibit superdiffusive motion – moving faster than random diffusion would predict – on intermediate timescales. “This work bridges materials science and biology,” says Smrek. “We’re showing that the same physics that governs synthetic polymers can explain behaviors in living systems. And it suggests we could design new materials that spontaneously develop directed transport properties,” adds Smrek. The findings open new avenues for creating functional active materials and provide a framework for interpreting chromatin dynamics experiments. They could further investigate how these effects combine with other active processes in biological systems and explore applications in smart materials that could transport cargo or heal themselves.
DISPOSABLE BABY DIAPERS RECYCLED INTO PYROLYSIS OILS TO PRODUCE NEW PLASTICS
N
Borouge International and BlueAlp are working with Woosh to chemically recycle disposable baby diapers into pyrolysis oils for producing new polymers. Consumption data suggests that 6.73 million metric tons of disposable diapers were generated in the EU-28 in 2017. These products are often incinerated or sent to a landfill after a single use, but Borouge points out that they contain ‘valuable’ polyolefin-based nonwovens and films. The collaboration builds on the pre-established ecosystem around Woosh’s giveback diapers, which are distributed to households and childcare facilities across Belgium, then collected again after use. Over 30,000 children are currently thought to use the system every day, with Woosh processing ‘thousands’ of metric tons of used diapers annually at its recently-launched diaper recycling plant. Woosh aims to expand its operations into France and the Netherlands to increase the volume of recovered plastic available for recycling. Engineers from Woosh have worked alongside Borouge International and BlueAlp to define the quality requirements of any recovered plastic to be used as input for BlueAlp’s chemical recycling technology. Woosh has adjusted its proprietary mechanical separation process accordingly. Initial industrial-scale recycling runs took place at BlueAlp’s plant in Oostende, Belgium. Its pyrolysis technology was used to process the recovered plastic fractions, converting them into ISCC PLUS-certified pyrolysis oil for future polymer production. This is thought to be the first time a circular economy has been established for single-use diapers at an industrial scale in Europe, and is intended as a proof of concept for circular systems in the sector. “Chemically recycling the plastic from used diapers is anything but straightforward,” explains Peter Voortmans, vice president Marketing Consumer Products at Borealis. “It requires careful pre-processing to meet the specifications of the pyrolysis process. “Together with Woosh and BlueAlp, we’ve been able to solve this challenge, showing what’s possible when teams work closely together with a shared goal.” “We have spent years building the collection network and the technology to make this possible,” continues Woosh CEO Jeff Stubbe. “To see the plastic we recover from used diapers validated as feedstock for new polymer production, and potentially for new diapers in the future, is exactly what we set out to achieve. This is what closing the loop actually looks like.” “This is a fundamental example of what we want to achieve at scale with BlueAlp,” adds BlueAlp CEO Valentijn de Neve. “It’s fantastic to see that, together, we can address difficultto-recycle waste streams that cannot be effectively managed through mechanical recycling, enabling them to be chemically recycled and returned to demanding applications such as diapers in the healthcare and hygiene sector.” Source: Packaging Europe – packagingeurope.com
The research was supported by the European Union through the QLUSTER project. Source: University of Vienna – www.univie.ac.at
Polímeros, 36(2), 2026
E5
E
W
S
A
G
E
N
D
2026 July 15th World Congress on Biopolymers and Biomaterials Date: July 27-28, 2026 Location: Paris, France Website: biopolymerscongress.conferenceseries.com 51st IUPAC World Polymer Congress (MACRO 2026) Date: July 28-31, 2026 Location: Sarawak, Malaysia Website: macro2026.org
August 12th International Conference on Chemical and Polymer Engineering (ICCPE 2026) Date: August 18-20, 2026 Location: London, United Kingdom Website: cpeconference.com 3rd Edition Global Summit on Polymer Science & Composite Materials Date: August 24-25, 2026 Location: Paris, France Website: globalpolysciencesummit.com FEIPLAR & FEIPUR 2026 – International Fair and Congress of Advanced Materials Date: August 25–27, 2026 Location: São Paulo, SP, Brazil Website: feiplar.com/en Interplast 2026 – Plastic Technology Exhibition & Congress Date: August 25–27, 2026 Location: Joinville, Santa Catarina, Brazil Website: interplast.com.br/en Global Summit on Sustainable Biopolymers and Polymer Applications (POLYMERS2026) Date: August 26-27, 2026 Location: Venice, Italy Website: biopolymers.researchconnects.org 11th International Conference on Research Innovations Trends in Macro Materials, Engineering, and Technology (SCOPUS) Date: August 28-29, 2026 Location: Manila, Philippines (hybrid) Website: socrd.org/icri-26/
September
A
Bioplastics Date: September 1-2, 2026 Location: Cleveland, Ohio, United States of America Website: ami-events.com/event/a57ba0e7-de68-4cf6-b4c58c0955be8ef5 International Conference on Macromolecular and Supramolecular Chemistry (ICMSC 2026) Date: September 14-15, 2026 Location: Zurich, Switzerland Website: waset.org/macromolecular-and-supramolecularchemistry-conference-in-september-2026-in-zurich International Conference on Polymer Chemistry and Molecular Engineering (ICPCAME-26) Date: September 16-17, 2026 Location: Cascais, Portugal Website: igaeglobal.com/conf/index.php?id=101066007 24th International Conference and Exhibition on Materials Science and Chemistry Date: September 21-22, 2026 Location: Barcelona, Spain Website: materialschemistry.chemistryconferences.org Annual Global Summit on Polymers and Composite Materials (AGSPOLYMERS2026) Date: September 21-23, 2026 Location: Prague, Czech Republic Website: vividglobalsummits.com/2026/composite-materials
E6
International Conference on Biopolymers and Polymers (ICBPS 2026) Date: September 23–24, 2026 Location: Berlin, Germany Website: polymers2026.pagesconferences.org/ XXVI International Symposium on Plastics Technology 2026 Date: September 23–24, 2026 Location: Campinas, São Paulo, Brazil Website: simposioplastico.com/en Global Polymer Summit Date: September 28–30, 2026 Location: Louisville, Kentucky, United States of America Website: gps2026.events.rubber.org International Conference on Next Horizons in Polymers: Beyond the past 50, toward the next 100 (IUPAC-PSK50) Date: September 28-October 1, 2026 Location: Busan, South Korea Website: polymer.or.kr/conferenceintl/default
October 5th International Conference on Polymer Science and Engineering Date: October 7-9, 2026 Location: San Francisco, California, United States of America Website: polymers.unitedscientificgroup.org 6th International Conference on Polymer Science & Composite Materials (ISTDPCM 2026) Date: October 15-16, 2026 Location: Dubai, United Arab Emirates Website: inovscitechconferences.com/2026/dubai/polymerscience XIX Latin American Symposium on Polymers and XVII Ibero-American Congress on Polymers - SLAP 2026 Date: October 19-23, 2026 Location: Salvador, Bahia, Brazil Website: slap2026.com.br 7th International Conference on Advanced Polymer Science and Engineering Date: October 26-28, 2026 Location: Madrid, Spain Website: polymersconference.yuktan.com
November Fire Resistance in Plastics Date: November 3-4, 2026 Location: Düsseldorf, Germany Website: ami-events.com/event/097c9771-7499-4a0c-9bb0d857a4ea771f Innovations in Plastics Recycling & Sustainability Date: November 8–11, 2026 Location: Santa Rosa, California, United States of America Website: polyacs.org/2026polyiprs PLASTIMAGEN® MEXICO 2026 Date: November 10–13, 2026 Location: Mexico City, Mexico Website: plastimagen.com.mx/en/ 3rd International Conference & Expo on Biopolymers, Polymer Science and Advanced Material (POLYMAT-2026) Date: November 26-28, 2026 Location: Munich, Germany Website: polymerscience.theinfiniteminds.net
December European Bioplastics Conference 2026 Date: December 1-2, 2026 Location: Berlin, Germany (Hybrid) Website:.european-bioplastics.org/events/ebc/ Polymer Engineering for Energy Date: December 1-2, 2026 Location: London, United Kingdom Website: ami-events.com/event/db799acb-6e78-46f4-9e3bd72992bb9495 PPS2026 – Asia/Australasia Regional Conference 2026 Date: December 1–4, 2026 Location: Phenikaa University, Duong Noi, Ha Noi, Viet Nam Website: pps2026.phenikaa-uni.edu.vn
Polímeros, 36(2), 2026
ABPol Associates Sponsoring Partners
Polímeros, 36(2), 2026
E7
ISSN 1678-5169 (Online)
https://doi.org/10.1590/0104-1428.20250092
Recent advances in natural fiber treatments for enhanced composite performance Mehmet Cihan1* , Marcos Antonio Gimenes Benega2 and Hélio Ribeiro3 Department of Naval Architecture and Marine Engineering, Fatsa Faculty of Marine Sciences, Ordu University, Fatsa, Ordu, Türkiye 2 Rheon Labs Ltd., London, United Kingdom 3 Escola de Engenharia, Universidade Presbiteriana Mackenzie, São Paulo, SP, Brasil
1
*mehmetcihan@odu.edu.tr
Abstract Natural fibers have attracted growing attention due to their sustainability, low cost, and low density, yet their hydrophilic nature limits compatibility with polymer matrices and constrains broader applications. To overcome this challenge, diverse surface modification techniques-including chemical, enzymatic, and physical treatments- have been developed to improve fiber–matrix interfacial adhesion. These modifications are crucial for significantly enhancing the mechanical performance and environmental robustness of the resulting composite materials.This review critically evaluates established and emerging strategies, highlighting their effectiveness, advantages, and limitations. Among the various approaches, alkali treatment remains the most widely adopted, demonstrating consistent improvements in composite performance through impurity removal, enhanced surface roughness, improved fiber–matrix adhesion, and superior load transfer capabilities. Keywords: chemical treatments, enzyme treatments, fiber-matrix interaction, natural fibers, physical treatments. Data Availability: All data supporting the findings of this study are available from the corresponding author upon request. How to cite: Cihan, M., Benega, M. A. G., & Ribeiro, H. (2026). Recent advances in natural fiber treatments for enhanced composite performance. Polímeros: Ciência e Tecnologia, 36(2), e20260016. https://doi.org/10.1590/0104-1428.20250092
1. Introduction The growing popularity of natural fibers is driven by increasing environmental awareness among consumers and industries, which has fueled demand for sustainable alternatives to synthetic materials[1,2]. Natural fibers, shown in Figure 1, offer biodegradability and often require less energy and water for production compared to their synthetic counterparts, aligning with global efforts towards a circular economy[3]. Their application spans a diverse range of areas, from automotive components and construction materials to marine structures and sporting equipment[4]. In the automotive sector, for instance, natural fiber composites are being explored as lightweight alternatives to traditional materials, contributing to fuel efficiency[3,5-7]. In civil engineering, they offer sustainable options for reinforcing concrete and other building materials[8-10]. Within the marine industry, they provide environmentally friendly alternatives for boat hulls and other structural elements[11,12]. Natural fibers offer several significant advantages, including sustainability, low density, resulting in comparable specific mechanical properties to E-glass fibers[13-15], desirable damping characteristics[16-18] and acoustical properties[19,20]. However, a range of inherent disadvantages limits their wider adoption. The hydrophilic nature of natural fibers renders their physical and mechanical properties susceptible
Polímeros, 36(2), e20260016, 2026
to fluctuations in environmental conditions, especially temperature and humidity[4,21-24]. This moisture sensitivity leads to dimensional instability, swelling, and reduced mechanical strength, particularly in humid environments. Furthermore, their poor compatibility with hydrophobic polymer matrices hinders the formation of strong interfacial bonds in composite materials[25]. The high hydrophilicity of natural fibers, a consequence of the numerous hydroxyl groups present in cellulose and the carboxyl acid groups within hemicellulose[30,31], contributes to increased water absorption and accelerated degradation, a key disadvantage compared to synthetic reinforcing fibers. However, synthetic fibers, typically hydrophobic polymers, exhibit significantly lower moisture absorption and are thus less susceptible to degradation in humid environments. This difference in hydrophilicity is a major factor limiting the widespread application of natural fibers in certain composite applications. The surface chemistry of natural fibers plays a crucial role in fiber-matrix interaction, as effective adhesion is a function of interfacial adhesion, chemical bonding, and mechanical interlocking[32]. While most natural fibers share common constituents such as cellulose, lignin, hemicellulose,
1/11
R R R R R R R R R R R R R R
Cihan, M., Benega, M. A. G., & Ribeiro, H. pectin, waxes, and ash[33], the relative proportions of these substances vary significantly depending on the fiber. For instance, flax fibers are characterized by a high wax and pectin content, whereas jute fibers exhibit a greater lignin content and lower pectin levels[34]. The presence of certain surface substances, such as waxes and oils, can hinder effective interaction with the matrix and thus necessitate their removal[34]. Given the distinct surface chemistry profiles of different fiber types, treatment techniques must be tailored to both the specific fiber and the chosen matrix. This targeted approach ensures optimal interfacial bonding and, consequently, enhances the mechanical properties of the resulting composite material. Furthermore, understanding these surface chemical variations is essential for developing effective surface modification strategies that promote stronger interfacial adhesion and improved composite performance. Numerous surface treatments, broadly categorized as chemical, enzymatic, and physical, have been developed.
Each of these categories includes a range of techniques that have been the subject of extensive research and schematic illustration of some of these techniques applied to natural fibers is depicted in Figure 2. This study aims to review recent advancements and discuss their implications for tailoring surface treatments to achieve optimal natural fiber reinforced composite performance.
2. Chemical Treatments The presence of hydroxyl groups on natural fibers renders them susceptible to chemical modification[35-37]. These hydroxyl groups can participate in intramolecular hydrogen bonding within cellulose, activating existing groups, or serve as reactive sites for the introduction of new chemical species that promote effective interlocking within the fiber structure. Chemical modification can thus be employed to tailor fiber surface characteristics, including wettability, adhesion, surface tension, and porosity[38,39]. Such modification can tailor the fibers interaction with different matrices, depending on their molecular affinity. Poor interfacial bonding, a consequence of the incompatibility between hydrophilic natural fibers and hydrophobic matrices, is a major challenge in composite manufacturing. Chemical treatments aim to mitigate these issues by reducing fiber hydrophilicity. By chemically removing water from the fibers, these treatments enhance fiber-matrix compatibility, leading to improved interfacial bonding and enhanced composite performance[40].
2.1 Acetylation
Figure 1. Classification of plant fibers[26-29].
The presence of hydroxyl (OH) groups in the cellulose and lignin components of natural fibers renders susceptible to moisture absorption. Acetylation, through reaction with acetyl (CH3CO) groups removes moisture by reacting with these hydroxyl groups. Tserki et al.[41] studied the effect of acetylation and propionylation treatments on hemp, flax and wood fibers. The results demonstrated that both treatments resulted in the removal of non-crystalline components, such
Figure 2. Graphical representation outlining several treatment techniques performed on a fiber. 2/11
Polímeros, 36(2), e20260016, 2026
Recent advances in natural fiber treatments for enhanced composite performance as waxy substances, from the fibers and induced changes in surface topography. Furthermore, the observed reduction in moisture adsorption suggests that esterification diminished the hydrophilicity of the materials. In another study conducted by Tserki et al.[42] suggested that acetylation and propionylation treatments resulted in improved stress transfer efficiency at the interface after optimization. Khalil et al.[43] studied effect of acetylation on interfacial shear strength (ISS) of oil palm empty fruit bunch (EFB) and coir fibers. Authors reported that acetylation of such fibers increased hydrophobicity, which in turn led to a significant improvement in ISS compared to unmodified fibers. This improved bonding is likely due to the altered fiber surface morphology caused by the acetylation process. The resulting hydrophobicity positively improved the compatibility with matrix materials. Zaman and Khan[44] studied the effect of acetylation treatment on the mechanical and dynamical properties of matted banana empty fruit bunch fiber (BBF), including tensile, flexural and impact strengths. It was concluded that acetylation-treated BBF reinforced composites exhibited reduced water absorption compared to both alkali-treated and untreated controls. Bledzki et al.[45] investigated the influence of acetylation on the structure and properties of flax fibers and their polypropylene composites. Acetylation resulted in a remarkable improvement in both the surface morphology and moisture resistance properties of flax fibers. It was claimed that depending on the degree of acetylation, flax fiber acetylation can reduce moisture absorption by up to 50%. The degree of acetylation was reported to have contrasting effects on the mechanical properties of the composites, increasing tensile and flexural strengths but decreasing Charpy impact strength.
2.2 Alkali treatment This process uses concentrated alkaline solutions, such as sodium hydroxide, to treat natural fibers, removing waxes, oils and other surface impurities from the fibers, thus increasing surface roughness that enhances mechanical interlocking[46], and enhancing mechanical bonding with the polymer matrix[47,48]. This process also reduces lignin and hemicellulose resulting in higher cellulose content and a cleaner fiber surface. However, optimal fiber properties depend on carefully controlling mercerization parameters, including alkali concentration, immersion time, temperature, and the specific type of fiber being treated[48]. Excessive sodium hydroxide (NaOH concentrations and prolonged exposure times can lead to the disintegration and dissolution of cellulose crystals[49]. Litaiff et al.[50] explored the utilization of mallow fibers as reinforcement in sustainable polymeric composites fabricated from bi-axially oriented polypropylene (BOPP) waste streams. To enhance interfacial bonding and mechanical performance, the authors subjected the fibers to alkali treatment. This surface modification proved highly effective, resulting in a substantial improvement in the fibers’ tensile characteristics: the treated fibers achieved a tensile strength of 1039.45 MPa, marking a significant increase over the 447.76 MPa exhibited by the untreated fibers, concurrent with a measured increase in the modulus of elasticity. Vishnu Vardhini et al.[51] investigated the influence of alkali treatment on the mechanical and impact properties Polímeros, 36(2), e20260016, 2026
of banana fiber-reinforced polypropylene composites. Specimens were treated with sodium hydroxide (NaOH) solutions at concentrations of 10%, 15%, and 20% to assess the impact of varying alkali concentrations on composite performance. Analysis of tensile properties revealed that all NaOH treatments positively influenced both tensile strength and tensile modulus. However, an optimal concentration of 15% NaOH was observed, beyond which (20% NaOH) a decrease in these properties was noted. Despite this decline at the highest concentration, specimens treated with 20% NaOH still exhibited superior tensile performance compared to those treated with the 10% solution. A similar trend emerged in impact testing, with specimens treated at 15% NaOH demonstrating the highest impact resistance, followed by those treated at 20% and 10%, respectively. This suggests that while increasing alkali concentration initially enhances impact properties, exceeding the optimal 15% concentration leads to a reduction, albeit not below the baseline established by the 10% treatment. In contrast to the tensile and impact behavior, flexural testing revealed a different trend. While the 15% NaOH treatment again yielded the highest performance, specimens treated with 10% NaOH exhibited superior flexural properties compared to those treated with the 20% solution. This indicates that for flexural properties, exceeding the optimal 15% concentration has a more detrimental effect, reducing performance below that achieved with the lowest concentration tested. Alkali treatment substantially improves the compatibility of coir fibers with polyvinyl alcohol/polyethylene glycol polymer blends, facilitating the production of composite films exhibiting superior mechanical properties[52]. Chamath et al. [53] claimed that removal of lignocellulosic constituents such as oil and wax, from the fiber surface increased with increasing alkali concentration. However, concentrations exceeding 4% NaOH induced surface damage, highlighting the critical balance required in alkaline treatment processes. Furthermore, improved thermal stability was observed in fibers treated with alkali concentrations up to 4% NaOH; beyond this threshold, further increases in concentration led to a reduction in thermal stability. These findings underscore the necessity for careful optimization of alkaline treatment parameters to achieve desired fiber properties. Consequently, a 4% NaOH concentration was determined to be optimal. The effect of alkaline treatment on the properties of bamboo/ coconut husk hybrid fibers was investigated by subjecting the fibers to NaOH solutions at concentrations ranging from 2% to 10%, the optimum concentration of NaOH was determined to be 8%[54]. Hafidz et al.[55] investigated the influence of alkaline treatment on the hygroscopic behavior of palm oil fibers and kenaf fibers reinforced unsaturated polyester composites, specifically examining water absorption and thickness swelling. They investigated the influence of 5% NaOH treatment on the water absorption characteristics of palm oil fiber/polyester and kenaf fiber/polyester composite samples at varying fiber volume fractions. In palm oil fiber composites, the 5% NaOH treatment resulted in a reduction in water absorption only at a 30% fiber volume fraction. At higher fiber volume fractions of 40% and 60%, the treatment did not yield any discernible improvement in water absorption behavior. In contrast, the kenaf fiber composites exhibited 3/11
Cihan, M., Benega, M. A. G., & Ribeiro, H. improved water absorption performance following the 5% NaOH treatment at both 30% and 40% fiber volume fractions. However, similar to the palm oil fiber composites, no improvement in water absorption was observed at the 60% fiber volume fraction. The influence of alkali treatment with a 5wt% NaOH for 30 minutes was investigated on linen, flax and bamboo fabric reinforced epoxy composites. Alkaline treatment resulted in substantial improvements in the tensile and flexural strength and modulus of all fabric-reinforced composites investigated. In contrast, the tensile and flexural strain of these composites increased only marginally, suggesting that the treatment primarily enhanced stiffness and load-bearing capacity rather than ductility or flexibility[56]. Prome et al.[57] investigated the optimization of natural fiber composites through a comparative study involving five distinct chemical treatments: Alkaline NaOH, Benzoyl Peroxide, Sodium Chlorite, Stearic Acid, and Potassium Permanganate. This methodology was applied to both banana fiber and JUCO (jute/cotton blend) composites. Significantly, the NaOH treated JUCO specimens demonstrated superior performance, achieving the highest recorded tensile strength 70.86 MPa and flexural strength 88.7 MPa under dry conditions. The dominant effect of NaOH treatment on jute fibers within epoxy composites was reported as fiber shrinkage[58]. This shrinkage was likely due to the removal of hemicellulose and other non-cellulosic components from the fiber structure during alkaline treatment, leading to a reduction in fiber diameter and potentially affecting fiber packing within the composite. The treatment also influenced the tensile properties and fracture mechanisms of the fibers, possibly through changes in cellulose crystallinity or microfibril orientation. However, despite these modifications to the fibers, no improvement in fiber-matrix adhesion was observed[58]. This lack of enhancement at the interface could be due to several factors, such as insufficient chemical bonding between the modified fiber surface and the epoxy matrix or the creation of a weak interfacial layer due to the removal of fiber components.
2.3 Silane treatment While silane coupling agents are extensively employed to enhance interfacial adhesion and mechanical properties in glass fiber-reinforced composites[59,60], their application
to natural fiber composites, including those reinforced with flax and kenaf fibers also demonstrated promising results[61]. The improvement in flax fiber-matrix compatibility achieved through silane treatment is attributed to the formation of hydrogen or covalent bonds between hydrolyzed silanol groups and the hydroxyl groups on the fiber surface. This enhanced interfacial bonding contributes to improved mechanical properties and reduced moisture sensitivity[62]. However, the effectiveness of silane treatment is influenced by factors such as the specific silane chemistry, fiber surface pretreatment, and processing conditions, which should be carefully considered for optimal performance[63,64]. The potential chemical coupling of GPS and PLA is shown in Figure 3. Various techniques for silane application to natural fibers have been documented. These techniques can be broadly classified into two categories: fiber surface treatment, which focuses on modifying the outer layer of the fiber, and cell wall modification, which targets deeper structural changes within the fiber[65]. The application of silane treatment to natural vegetable fibers yielded enhancements in both Young’s modulus and tensile strength. Additionally, a reduction of approximately 60% in the moisture absorption of the resulting composites was observed[66]. Silane treatment also improves the compatibility between hydrophilic fibers and hydrophobic polymer matrices by modifying the fiber surface with silane coupling agents. However, silane coupling agents are more expensive than common NaOH for alkali treatment and can be more expensive than plasma treatment in large scale manufacturing. Its effectiveness is also dependent upon factors such as the specific silane agent used and its concentration[67]. Rothenhäusler et al.[68] investigated the influence of various treatments, namely: Sodium hydroxide (NaOH) (alkali), silane and siloxane treatments. Flax fiber-reinforced composites manufactured with alkali treated fibers outperformed all other modifications examined, including composites reinforced with untreated flax fibers. This enhancement in mechanical properties is attributed to the alterations in fiber composition, coupled with improved fiber-matrix adhesion. The improved adhesion was achieved through the removal of the thermoplastic binder and the creation of a rougher fiber surface. Conversely, neither silane nor siloxane modifications yielded improvements in composite tensile properties relative to untreated controls. Another
Figure 3. Potential chemical coupling of GPS and PLA[59]. 4/11
Polímeros, 36(2), e20260016, 2026
Recent advances in natural fiber treatments for enhanced composite performance study demonstrating the ineffectiveness of silane treatment on the natural fibers was published by John and Naidu[69] who investigated effect of alkali and silane treatments on the flexural properties of hybridized sisal and E-glass fibers. The results indicated that silane treatment did not significantly affect the flexural properties, whereas alkali treatment led to a marginal improvement in these properties.
2.4 Benzyl treatment Benzoylation is another method used to increase the fiber’s affinity to non-polar resins, thus enhancing adhesion. The interaction between the hydroxyl functionalities of the cellulose fiber and benzoyl chloride, resulting in a specific chemical reaction, is depicted in Figure 4. Zulyadain et al.[70] prepared composites from PLA and benzoylated sugarcane bagasse at different loads of treated and untreated fiber loads. Their results showed improvement in tensile strength and elongation, notably between 5 and 10% fiber loading. The modulus at break was more consistent for the treated fibers, but at fiber loads below 15%, the modulus was lower than the untreated fibers. The impact performance was overall higher for the treated fibers. Jiyas et al.[72] studied the effect of different benzoylation reaction times on bamboo fibers. They compared the results with untreated fibers and those only treated with NaOH. Though not in a composite system, their work showed that benzoylation improved the fibers’ properties. The best improvements were progressive up to 15 min reaction time. At 20 min, all the properties were lower than 15%. This behavior was shown in water content, water absorption, tensile stress and tensile modulus. Izwan et al.[73] prepared polypropylene composites with small (0.1 to 0.5 mm) benzoylated kenaf and sugar palm fibers. In their study, a hybrid system was created by adding 10% of a mixture of the two fibers (3:7, 5:5 and 7:3). These fiber loadings were compared to the same loadings of untreated fibers. Treated fibers showed higher glass transition temperatures and melting points, especially for 5:5. However, the addition of small fibers to polypropylene reduced the flexibility and damping capacity of the composites. Sahu et al. [3] study showed that benzoylation yielded the highest content of cellulose and lowest content of hemicellulose and lignin in Bauhinia vahlii fibers. Benzoylated fibers also presented the highest tensile strength, Young’s modulus and crystallinity index. They concluded that benzoylation was the preferred method when comparing to alkali and bleaching treatments. A research conducted by Dipta et al.[74] focused on statistically characterizing the ultimate tensile strength of Talipot Palm Fiber (TPF), thereby addressing the inherent mechanical data scatter common in natural reinforcements. The experimental regime involved subjecting the fibers to
three distinct chemical modifications- alkalization NaOH, acetylation, and benzylation-each systematically evaluated across three concentration levels (5%, 10%, and 15% by weight). All treatments significantly enhanced the ultimate tensile strength compared to the raw fibers, a finding supported by XRD and FTIR analyses that confirmed the successful removal of amorphous hemicellulose and lignin. The optimal enhancement was achieved using the 10% NaOH concentration, which yielded the highest recorded tensile strength of 462.47 MPa, whilst the 5% benzylated Talipot Palm Fiber exhibited the lowest ultimate tensile strength. Crucially, the study observed that concentrations exceeding this 10% threshold resulted in diminished tensile strength, indicating that excessive chemical exposure induced structural degradation of the cellulosic crystalline chains.
2.5 Maleated coupling agents Maleation treatment involves the application of a coupling agent to both the fiber surface and the polymer matrix. This process typically involves grafting maleic anhydride onto the polymer to enhance compatibility between the coupling agent and the matrix[75]. The incorporation of maleic anhydride is crucial for improving interfacial adhesion between the fiber and the matrix. During the grafting process, maleic anhydride reacts with hydroxyl groups present on the fiber surface, effectively reducing their availability for other interactions[76]. The interaction between the anhydride groups of maleated coupling agents and the hydroxyl groups present on natural fibers effectively addresses the issue of incompatibility, leading to enhanced tensile and flexural strengths in natural fiber thermoplastic composites[77]. Maleated polypropylene (MAH-PP) reacts with the hydroxyl groups significantly enhanced the composites’ mechanical properties under both tensile and flexural stress. This improvement is attributed to covalent bonding between the natural fibers’ surface hydroxyl groups and the maleic anhydride in MAH-PP[78]. El-Sabbagh[79] investigated the optimum maleic anhydride polypropylene (MAPP) ratio to natural fibers; namely flax, hemp and sisal fibers. Fibers were pretreated by NaOH at various ratios. The optimal ratio of MAPP for natural fibers varied between 10% and 13.3%, depending on both the specific MAPP source and the type of natural fiber used, as well as the mechanical property being evaluated namely, stiffness, impact and strength[79].
3. Enzyme Treatments A variety of enzymes can be used in enzyme treatment, but cellulase, xylanase, and pectinase are particularly prevalent due to their effectiveness in modifying plant-based materials. Enzymatic treatment effectively removes hygroscopic pectic
Figure 4. Reaction scheme of a benzoylated fiber[71]. Polímeros, 36(2), e20260016, 2026
5/11
Cihan, M., Benega, M. A. G., & Ribeiro, H. and hemicellulosic substances, resulting in more uniform fiber surfaces with enhanced thermal properties. Enzymes improve the thermal stability of natural fibers by selectively removing less stable pectic and hemicelluloses[80]. Flax and hemp fibers were treated with five different enzymes, namely: xylanase, xylanase+cellulase, polygalacturonase, pectinmethylesterase and laccase. Enzymatic treatment was more efficient on flax fibers than on hemp fibers due to flax fibers’ greater surface area[80]. Jute fibers were treated with enzymes (pectinase, laccase, xylanase, and cellulase) to assess the impact of enzymatic pretreatment on the mechanical properties of jute/polyester composites[81]. Enzymatic treatment caused fabric fibrillation and yarn opening, resulting in a hairier fabric due to the removal of adhesive substances such as hemicelluloses, lignin, pectin, and oils. This increased surface area led to a stronger fiber-matrix interaction and improved adhesion with the polyester matrix[81]. Natural fibers are not only utilized in composite materials but also in clothing, and textiles. Similar enzyme treatments are employed to achieve different objectives. For instance, enzymatic treatments can enhance the whiteness of fiber surfaces, improving their aesthetic appeal. However, this often involves a trade-off: while desired physical characteristics, such as increased brightness or improved dyeability, are achieved, the fiber’s mechanical properties, such as tensile strength or flexibility, may be compromised. Enzyme concentration had a pronounced effect on both the mechanical and physical attributes of jute fibers[82]. Specifically, increasing the enzyme concentration weakened the flexural rigidity, likely due to the enzymatic breakdown of structural components. Conversely, this increase in the enzyme concentration enhanced physical properties related to appearance, such as brightness index, whiteness index, and reflectance, potentially by removing impurities or surface coatings. In a study by Zwane et al.[83], investigated the impact of enzymatic treatment on the tensile strength and morphology of sisal fibers. Their goal was to explore hemicellulose, an enzyme derived from Aspergillus niger, as an alternative method to hydrolyze the cementing layers within sisal fibers. Conversely, their findings diverged from previous studies on natural fibers, which often report positive effects of enzymatic treatment. Zwane et al.[83] observed that both sodium hydroxide (NaOH) and enzymatic treatments resulted in a decrease in the tensile properties of the fibers. Vishnu Vardhini et al.[51] investigated the influence of enzymatic treatments on the tensile strength, flexural strength, and impact resistance of banana fiber/polypropylene composites. The enzymes employed were laccase and xylanase, applied at concentrations of 10%, 15%, and 20% to assess the impact of varying enzyme concentration on composite mechanical properties. Regarding tensile properties, xylanase treatment exhibited a more pronounced effect than laccase. A maximum increase of approximately 70% in tensile strength was achieved with xylanase at the 20% concentration, representing the highest value observed across all xylanase concentrations tested. Laccase treatment, at the same 20% concentration, resulted in an approximate 56% increase in tensile strength. A similar trend was observed in 6/11
flexural properties. Xylanase treatment induced an increase of over 100% in flexural strength at the 20% concentration, while laccase treatment at the same concentration yielded an 86% increase. This again demonstrates the superior effect of xylanase treatment on the flexural behavior of the composites. The impact of xylanase treatment was particularly notable in terms of impact strength, achieving an improvement exceeding 120%. While laccase-treated samples also demonstrated substantial improvement, they achieved a slightly lower increase of approximately 114%. This further reinforces the observation that xylanase treatment had a greater positive impact on the mechanical properties of the banana fiber/polypropylene composites compared to laccase treatment under the conditions investigated.
4. Physical Treatments A variety of physical modification techniques have been documented, aimed at altering the surface properties of materials. These methods can be broadly classified into radiative and electrical discharge approaches. Radiation methods, including X-rays, ionizing radiation, gamma radiation, induce surface modifications by altering the chemical composition and morphology through high-energy interactions[84,85]. Electrical discharge methods, such as plasma, corona discharges and so on.
4.1 Corona discharge Corona discharge treatment has emerged as a promising alternative to conventional pretreatment methods due to its environmentally friendly nature and suitability for industrial processes, offering economic advantages[86,87]. This method modifies plant fiber surfaces by activating the constituent polymers, which leads to improvements in both wettability and adhesion strength[88]. Corona pretreatment enhances fiber-matrix adhesion by activating the fiber surface and increasing its roughness. The surface activation is likely a result of the corona discharge generating reactive species that interact with the fiber surface, potentially creating carboxyl, hydroxyl, or other polar functional groups. These newly formed groups can then form stronger chemical bonds with the matrix, while the increased surface roughness provides additional sites for mechanical interlocking, leading to improved overall adhesion[89]. Corona discharge treatments enhanced the fiber-matrix adhesion of jute/polyester composites[90], however, the application of corona discharge treatment to jute fibers resulted in a reduction in tensile strength, which ultimately led to a decrease in the mechanical performance of the jute fiber/ epoxy composites[89]. Corona discharge treatment constitutes a vital step in textile processing[91]. The widespread adoption of this technique is largely attributable to its economic feasibility, stemming from its low energy demand and inherently low operational cost.
4.2 Plasma treatment Plasma treatment is a versatile technique capable of generating both rough and smooth surface morphologies. Furthermore, it allows for the modification of the substrate’s chemical composition through the introduction of diverse Polímeros, 36(2), e20260016, 2026
Recent advances in natural fiber treatments for enhanced composite performance functional groups. This dual capability makes plasma treatment a powerful tool in various applications, including enhancing adhesion in composite materials, improving the wettability of surfaces for coating applications[92]. Plasma surface modification offers both economic and ecological advantages[93] by eliminating the need for water and chemicals[94]. A significant benefit of plasma processing is the substantial reduction in pollutant generation, leading to a corresponding decrease in effluent treatment costs[95]. Consequently, plasma treatment can be considered an environmentally friendly technology. Plasma treatment physically modifies the fiber surface, creating roughness through a sputtering process[96]. This surface roughening increases the contact area available for interaction with the polymer, resulting in enhanced interfacial friction. The mechanical properties of jute fibers and their PLA composites were studied as a function of plasma treatment exposure time[95]. Plasma treatment proved highly effective in enhancing the mechanical properties of jute fiber-reinforced composites. Significant increases were observed across all measured properties: tensile strength increased by 28%, Young’s modulus by 17%, and flexural strength by 20%. Notably, the flexural strength of the treated composites exceeded that of the untreated composites by over 20%. This substantial improvement in flexural performance, along with the gains in tensile strength and modulus, suggests a marked enhancement in interfacial adhesion between the jute fibers and the PLA matrix due to the plasma treatment. Following plasma treatments, significant changes were observed in the surface chemistry of the flax fibers, including alterations in functional group composition and an increase in surface roughness[97]. The most notable observation was the generation of new functional groups, indicating a chemical interaction between the plasma and the fiber surface.
5. Discussion and Conclusion The increasing utilization of natural fiber-reinforced composites offers a promising avenue for significant enhancements in component quality across multiple critical dimensions. Specifically, these materials present substantial advantages with respect to environmental impact, offering the potential for reduced reliance on non-renewable resources. Furthermore, their economic viability is emphasized by the potential for lower raw material costs and reduced energy consumption during processing in certain applications. From a technical feasibility standpoint, these composites can provide tailored mechanical properties, including acceptable strength-to-weight ratios and damping characteristics, making them suitable for a widening range of engineering applications. However, their inherited limitations keep them away from a wider range of use in multiple industries. Surface treatments play a crucial role in enhancing the performance of natural fibers in advanced composites by addressing their inherent limitations of high moisture absorption and poor dimensional stability. The principal mechanistic underpinnings of the current treatment methodologies can be summarized as follows: -
Acetylation effectively mitigates the inherent moisture sensitivity of natural fibers by chemically substituting
Polímeros, 36(2), e20260016, 2026
the hydrophilic hydroxyl groups within cellulose and lignin, thereby reducing the fiber hydrophobicity. -
Alkali treatment stands out as a vital surface modification technique for natural fibers. It optimizes composite performance by purifying and etching the fiber surface, thereby promoting superior fiber-matrix adhesion, efficient stress transfer, and enhanced mechanical properties.
-
Silane treatment enhances flax fiber-matrix compatibility by fostering interfacial hydrogen or covalent bonding between hydrolyzed silanol and fiber surface hydroxyl groups. This improved interfacial adhesion consequently leads to enhanced mechanical performance and reduced moisture sensitivity of the resulting composites.
-
Benzoylation represents an effective chemical modification strategy for enhancing the interfacial adhesion between cellulose fibers and non-polar resin matrices. This improvement is achieved through a specific chemical reaction, namely the esterification of the fiber’s hydroxyl functionalities by benzoyl chloride, thereby increasing the fiber’s affinity for the hydrophobic resin.
-
Maleation treatment, employing a coupling agent on both the fiber and polymer matrix, typically involves grafting maleic anhydride onto the polymer to enhance matrix compatibility. This incorporation of maleic anhydride is critical for improving fiber-matrix interfacial adhesion by reacting with hydroxyl groups on the fiber surface during the grafting process, thereby modulating their reactivity.
-
Enzymatic treatment effectively enhances the thermal properties of natural fibers by selectively removing hygroscopic pectic and hemicellulosic components, resulting in more uniform surfaces and improved thermal stability.
-
Corona treatment is shown to bolster fiber-matrix adhesion via dual mechanisms: the generation of polar functional groups on the fiber surface enhances chemical bonding, and roughening improves mechanical interlocking with the matrix.
-
Plasma treatment stands as a versatile methodology, enabling precise control over both surface topography and chemical functionality. This dual capability positions plasma technology as a powerful and adaptable tool across a spectrum of applications, enhancing interfacial adhesion in composite systems and optimizing surface wettability for coating processes.
Finally, this review highlighted the main strategies currently employed for natural fiber treatments; nevertheless, alternative techniques remain underexplored and deserve further attention in future studies.
6. Author’s Contribution • Conceptualization – Mehmet Cihan. • Data curation – NA. • Formal analysis – NA. • Funding acquisition - NA. • Investigation – Mehmet Cihan. 7/11
Cihan, M., Benega, M. A. G., & Ribeiro, H. • Methodology – Mehmet Cihan. • Project administration – Mehmet Cihan. • Resources – Mehmet Cihan. • Software – NA. • Supervision – NA. • Validation – NA. • Visualization – Mehmet Cihan; Marcos Antonio Gimenes Benega. • Writing – original draft – Mehmet Cihan; Marcos Antonio Gimenes Benega. • Writing – review & editing – Mehmet Cihan; Marcos Antonio Gimenes Benega; Hélio Ribeiro.
7. Acknowledgements The authors thank the Coordination for the Improvement of Higher Education Personnel–Brazil (CAPES)-PRINT Grant: 88887.310339/2018-00, Mackenzie Research Fund (Mackpesquisa, Project number 231015). The authors also thank the Conselho Nacional de Desenvolvimento Científico e Tecnológico (CNPq, Brazil, grant number 303139/20242) and the Fundação de Amparo à Pesquisa do Estado de São Paulo (FAPESP, Brazil, grant number 2023/08110-1).
8. References 1. Sankar Lal, S., Kannan, S., & Sahoo, S. K. (2022). Influence of flax fiber orientation on mechanical, thermo-mechanical and interfacial adhesion properties of epoxidized methyl ricinoleate modified epoxy composite: A sustainable green composite for cleaner production. Materials Today. Communications, 33, 104648. https://doi.org/10.1016/j.mtcomm.2022.104648. 2. Khatami, M., Bairwan, R. D., Khalil, H. P. S. A., Surya, I., Mawardi, I., Ahmad, A., & Yahya, E. B. (2024). The role of natural fiber reinforcement in thermoplastic elastomers biocomposites. Fibers and Polymers, 25(8), 3061-3077. https:// doi.org/10.1007/s12221-024-00621-5. 3. Sahu, D. P., Kumar, S., & Gupta, M. K. (2025). Flexural and free vibration analysis of glass and natural fiber-based hybrid laminated composites: experimental and numerical insights. Fibers and Polymers, 26(4), 1765-1782. https://doi.org/10.1007/ s12221-025-00902-7. 4. Chen, J., Lei, L., Ji, C., Yang, S., Cheng, Z., Fan, J., & Yu, T. (2025). Cluster analysis of acoustic emission signals for bending damage mechanism of flax fiber reinforced composites under hydrothermal aging. Composites Communications, 53, 102165. https://doi.org/10.1016/j.coco.2024.102165. 5. Volpe, V., & Pantani, R. (2025). Natural fiber-reinforced light composites for the automotive industry. Polymer Composites, 46(9), 8660-8673. https://doi.org/10.1002/pc.29518. 6. Neto, J., Queiroz, H., Aguiar, R., Lima, R., Cavalcanti, D., & Banea, M. D. (2022). A review of recent advances in hybrid natural fiber reinforced polymer composites. Journal of Renewable Materials, 10(3), 561-589. https://doi.org/10.32604/ jrm.2022.017434. 7. Ullah, S., Akhter, Z., Palevicius, A., & Janusas, G. (2025). Review: natural fiber-based biocomposites for potential advanced automotive applications. Journal of Engineered Fibers and Fabrics, 20, 15589250241311468. https://doi. org/10.1177/15589250241311468. 8. Veerappan, P., Mani, I., John, A., & Madhavan, H. (2024). Experimental studies of coir and jute-fiber reinforced 8/11
concrete with M-sand. Matéria, 29(2), e20240115. https:// doi.org/10.1590/1517-7076-rmat-2024-0115. 9. Joachim, L., & Oettel, V. (2024). Experimental investigations on the application of natural plant fibers in ultra-high-performance concrete. Materials, 17(14), 3519. https://doi.org/10.3390/ ma17143519. PMid:39063811. 10. Awoyera, P. O., Akin-Adeniyi, A., Althoey, F., Abuhussain, M. A., Jolayemi, K., & Romero, L. M. B. (2024). Green structural retrofitting materials for fire-damaged reinforced concrete buildings: advances in sustainable repair of distressed buildings. Fire Technology, 60(3), 1955-1991. https://doi.org/10.1007/ s10694-024-01557-1. 11. Putra, N. R., Ismail, A., Sari, D. P., Suwahyu, S., Utina, M. R., Rizal, N., Machfudin, A., Sandjaja, I. E., & Pratikno, H. (2025). Innovations and trends in composite materials for maritime applications: a 2000–2024 bibliometric study and comprehensive review. Ships and Offshore Structures, 0, 1-18. https://doi.org/10.1080/17445302.2025.2455987. 12. Baley, C., Davies, P., Troalen, W., Chamley, A., Dinham-Price, I., Marchandise, A., & Keryvin, V. (2024). Sustainable polymer composite marine structures: developments and challenges. Progress in Materials Science, 145, 101307. https://doi. org/10.1016/j.pmatsci.2024.101307. 13. Sakoshev, Z. G., Blaznov, A. N., Bychin, N. V., Medvedev, P. A., Zadvornykh, G. S., Sakoshev, E. G., Firsov, V. V., & Cheremukhina, I. V. (2024). Morphological and physicomechanical characterization of synthetic and natural fibers. Journal of Polymer Research, 31(3), 86. https://doi.org/10.1007/s10965024-03938-0. 14. Ravishankar, P., Arya, M., Dhakal, H., Gouda, F., Skrifvars, M., & Khalili, P. (2024). Assessing the mechanical performance of natural fiber thermoplastic composite sandwiches for advanced applications. Results in Materials, 23, 100600. https://doi. org/10.1016/j.rinma.2024.100600. 15. Blanchard, J. M. F. A., Sobey, A. J., & Blake, J. I. R. (2016). Multi-scale investigation into the mechanical behaviour of flax in yarn, cloth and laminate form. Composites. Part B, Engineering, 84, 228-235. https://doi.org/10.1016/j. compositesb.2015.08.086. 16. Nema, A., Penumakala, P. K., & Adusumalli, R. B. (2025). Dynamic mechanical analysis of flax / carbon hybrid composites : experimental and theoretical investigation. Materials Today. Communications, 43, 111770. https://doi.org/10.1016/j. mtcomm.2025.111770. 17. Cihan, M., Sobey, A. J., & Blake, J. I. R. (2019). Mechanical and dynamic performance of woven flax/E-glass hybrid composites. Composites Science and Technology, 172, 36-42. https://doi.org/10.1016/j.compscitech.2018.12.030. 18. Li, Q., Li, Y., Ma, H., Cai, S., & Huang, X. (2020). Effect of processing temperature on the static and dynamic mechanical properties and failure mechanisms of flax fiber reinforced composites. Composites Communications, 20, 100343. https:// doi.org/10.1016/j.coco.2020.04.009. 19. Merotte, J., Le Duigou, A., Bourmaud, A., Behlouli, K., & Baley, C. (2016). Mechanical and acoustic behaviour of porosity controlled randomly dispersed flax/PP biocomposite. Polymer Testing, 51, 174-180. https://doi.org/10.1016/j. polymertesting.2016.03.002. 20. Satankar, R. K., Sharma, N., Katariya, P. V., Kumar, V., Dewangan, H. C., Pal, A., & Panda, S. K. (2023). Computational modelling and analysis of thermoacoustic behaviour of carbon nanotube-reinforced plant fibre epoxy composite – An extensive review. Materials Today. Communications, 36, 106717. https:// doi.org/10.1016/j.mtcomm.2023.106717. 21. Le Duigou, A., Davies, P., & Baley, C. (2013). Exploring durability of interfaces in flax fibre/epoxy micro-composites. Polímeros, 36(2), e20260016, 2026
Recent advances in natural fiber treatments for enhanced composite performance Composites. Part A, Applied Science and Manufacturing, 48, 121-128. https://doi.org/10.1016/j.compositesa.2013.01.010. 22. Moudood, A., Rahman, A., Khanlou, H. M., Hall, W., Öchsner, A., & Francucci, G. (2019). Environmental effects on the durability and the mechanical performance of flax fiber/bioepoxy composites. Composites. Part B, Engineering, 171, 284-293. https://doi.org/10.1016/j.compositesb.2019.05.032. 23. Seisa, K., Chinnasamy, V., & Ude, A. U. (2022). Surface treatments of natural fibres in fibre reinforced composites: a review. Fibres & Textiles in Eastern Europe, 30(2), 82-89. https://doi.org/10.2478/ftee-2022-0011. 24. Yang, S., Chen, J., Lei, L., Cheng, Z., Yu, T., Fan, J., Du, J., Li, Q., & Yang, W. (2025). Unlocking the fungi aging secrets of sisal fiber reinforced polylactic acid composites. Composites Communications, 55, 102296. https://doi.org/10.1016/j. coco.2025.102296. 25. Cihan, M., Benega, M. A. G., & Ribeiro, H. (2022). Investigating the moisture content of flax fibre reinforced composite materials. Turkish Journal of Maritime and Marine Sciences, 8(2), 161-166. https://doi.org/10.52998/trjmms.1144083. 26. Skosana, S. J., Khoathane, C., & Malwela, T. (2024). Driving towards sustainability: A review of natural fiber reinforced polymer composites for eco-friendly automotive light-weighting. Journal of Thermoplastic Composite Materials, 38(2), 754-780. https://doi.org/10.1177/08927057241254324. 27. Shakir, M. H., & Singh, A. K. (2024). Ramie fiber and its composites: A review. Polymer Composites, 46(8), 6813-6841. https://doi.org/10.1002/pc.29417. 28. Fuqua, M. A., Huo, S., & Ulven, C. A. (2012). Natural fiber reinforced composites. Polymer Reviews (Philadelphia, Pa.), 52(3), 259-320. https://doi.org/10.1080/15583724.2012.7054 09. 29. Biagiotti, J., Puglia, D., & Kenny, J. M. (2004). A review on natural fibre-based composites-Part I. Journal of Natural Fibers, 1(2), 37-68. https://doi.org/10.1300/J395v01n02_04. 30. Farhat, W., Venditti, R. A., Hubbe, M., Taha, M., Becquart, F., & Ayoub, A. (2017). A review of water-resistant hemicellulosebased materials: processing and applications. ChemSusChem, 10(2), 305-323. https://doi.org/10.1002/cssc.201601047. PMid:28029233. 31. Feng, Y., Hao, H., Lu, H., Chow, C. L., & Lau, D. (2024). Exploring the development and applications of sustainable natural fiber composites: A review from a nanoscale perspective. Composites. Part B, Engineering, 276, 111369. https://doi. org/10.1016/j.compositesb.2024.111369. 32. Tran, L. Q. N., Fuentes, C. A., Dupont-Gillain, C., Van Vuure, A. W., & Verpoest, I. (2013). Understanding the interfacial compatibility and adhesion of natural coir fibre thermoplastic composites. Composites Science and Technology, 80, 23-30. https://doi.org/10.1016/j.compscitech.2013.03.004. 33. Chokshi, S., Parmar, V., Gohil, P., & Chaudhary, V. (2022). Chemical composition and mechanical properties of natural fibers. Journal of Natural Fibers, 19(10), 3942-3953. https:// doi.org/10.1080/15440478.2020.1848738. 34. Nassar, M. M. A., Alzebdeh, K. I., Al-Hinai, N., & Pervez, T. (2023). A new multistep chemical treatment method for high performance natural fibers extraction. Journal of Natural Fibers, 20(1), 2150922. https://doi.org/10.1080/15440478.2 022.2150922. 35. Pinto, Â., Esteves, D., Nobre, L., Bessa, J., Cunha, F., & Fangueiro, R. (2025). Mechanical performance enhancement in natural fibre-reinforced thermoplastic composites through surface treatment and matrix functionalisation. Polymers, 17(4), 532. https://doi.org/10.3390/polym17040532. PMid:40006192. 36. Aravinth, K., Ramakrishnan, T., Tamilarasan, V. D., & Veeramanikandan, K. (2022). A brief review on plant fibres Polímeros, 36(2), e20260016, 2026
composites: Extraction, chemical treatment and fibre orientation. Materials Today: Proceedings, 62(Part 4), 2005-2009. https:// doi.org/10.1016/j.matpr.2022.02.291. 37. Ganguly, A., Shankar, S., Das, A., Shukla, M., Swaroop, C., & Bhardwaj, T. (2022). Natural fibre reinforced composites: A review based on additive manufacturing routes and biodegradability perspective. Materials Today: Proceedings, 62(Part 1), 131135. https://doi.org/10.1016/j.matpr.2022.02.607. 38. John, M. J., & Anandjiwala, R. D. (2008). Recent developments in chemical modification and characterization of natural fiberreinforced composites. Polymer Composites, 29(2), 187-207. https://doi.org/10.1002/pc.20461. 39. Baley, C., Busnel, F., Grohens, Y., & Sire, O. (2006). Influence of chemical treatments on surface properties and adhesion of flax fibre-polyester resin. Composites. Part A, Applied Science and Manufacturing, 37(10), 1626-1637. https://doi. org/10.1016/j.compositesa.2005.10.014. 40. Kabir, M. M., Wang, H., Lau, K. T., & Cardona, F. (2012). Chemical treatments on plant-based natural fibre reinforced polymer composites: an overview. Composites. Part B, Engineering, 43(7), 2883-2892. https://doi.org/10.1016/j. compositesb.2012.04.053. 41. Tserki, V., Zafeiropoulos, N. E., Simon, F., & Panayiotou, C. (2005). A study of the effect of acetylation and propionylation surface treatments on natural fibres. Composites. Part A, Applied Science and Manufacturing, 36(8), 1110-1118. https:// doi.org/10.1016/j.compositesa.2005.01.004. 42. Tserki, V., Panayiotou, C., & Zafeiropoulos, N. E. (2005). A study of the effect of acetylation and propionylation on the interface of natural fibre biodegradable composites. Advanced Composites Letters, 14(2), 096369350501400202. https://doi. org/10.1177/096369350501400202. 43. Khalil, H. P. S. A., Ismail, H., Rozman, H. D., & Ahmad, M. N. (2001). The effect of acetylation on interfacial shear strength between plant fibres and various matrices. European Polymer Journal, 37(5), 1037-1045. https://doi.org/10.1016/ S0014-3057(00)00199-3. 44. Zaman, H. U., & Khan, R. A. (2021). Acetylation used for natural fiber/polymer composites. Journal of Thermoplastic Composite Materials, 34(1), 3-23. https://doi.org/10.1177/0892705719838000. 45. Bledzki, A. K., Mamun, A. A., Lucka-Gabor, M., & Gutowski, V. S. (2008). The effects of acetylation on properties of flax fibre and its polypropylene composites. Express Polymer Letters, 2(6), 413-422. https://doi.org/10.3144/expresspolymlett.2008.50. 46. Valadez-Gonzalez, A., Cervantes-Uc, J. M., Olayo, R., & Herrera-Franco, P. J. (1999). Effect of fiber surface treatment on the fiber-matrix bond strength of natural fiber reinforced composites. Composites. Part B, Engineering, 30(3), 309-320. https://doi.org/10.1016/S1359-8368(98)00054-7. 47. Sahu, P., & Gupta, M. K. (2020). A review on the properties of natural fibres and its bio-composites: effect of alkali treatment. Proceedings of the Institution of Mechanical Engineers. Proceedings Part L, Journal of Materials: Design and Applications, 234(1), 198-217. https://doi.org/10.1177/1464420719875163. 48. Luchese, C. L., Engel, J. B., & Tessaro, I. C. (2024). A review on the mercerization of natural fibers: parameters and effects. Korean Journal of Chemical Engineering, 41(3), 571-587. https://doi.org/10.1007/s11814-024-00112-6. 49. Bartos, A., Anggono, J., Farkas, Á. E., Kun, D., Soetaredjo, F. E., Móczó, J., Antoni, A., Purwaningsih, H., & Pukánszky, B. (2020). Alkali treatment of lignocellulosic fibers extracted from sugarcane bagasse: Composition, structure, properties. Polymer Testing, 88, 106549. https://doi.org/10.1016/j. polymertesting.2020.106549. 50. Litaiff, H. A., Santos, G. M. D., Melo, G. D., Cunha, C. D., & Giacon, V. M. (2025). Influence of alkali treatment on physical9/11
Cihan, M., Benega, M. A. G., & Ribeiro, H. mechanical properties of mallow fiber/BOPP composites. Polímeros, 35(1), e20250006. https://doi.org/10.1590/01041428.20240040. 51. Vishnu Vardhini, K. J., Murugan, R., & Surjit, R. (2018). Effect of alkali and enzymatic treatments of banana fibre on properties of banana/polypropylene composites. Journal of Industrial Textiles, 47(7), 1849-1864. https://doi.org/10.1177/1528083717714479. 52. Vandna, V., & Yadav, V. L. (2024). Influence of alkali treatment on coir-reinforced polyvinyl alcohol/polyethylene glycol blends. Journal of Plastic Film & Sheeting, 40(3), 307-327. https://doi.org/10.1177/87560879241255892. 53. Chamath, L. G., Srimal, L. K. T., Sewvandi, G. A., Gallage, R., & Epaarachchi, J. (2025). Optimizing the alkaline concentration for coir fibre treatment and estimation of lifetime. Journal of the National Science Foundation of Sri Lanka, 52(4), 515-525. https://doi.org/10.4038/jnsfsr.v52i4.12098. 54. Sapiee, N. H. (2024). Influence of alkali treatment on bamboo/ coconut husk hybrid fibre polyester composite. Jixie Gongcheng Xuebao, 21(2), 107-124. https://doi.org/10.24191/jmeche. v21i2.26258. 55. Hafidz, N. S. B. M., Rehan, M. S. B. M., & Mokhtar, H. B. (2021). Effect of alkaline treatment on water absorption and thickness swelling of natural fibre reinforced unsaturated polyester composites. Materials Today: Proceedings, 48(Part 4), 720-727. https://doi.org/10.1016/j.matpr.2021.02.209. 56. Yan, L., Chouw, N., & Yuan, X. (2012). Improving the mechanical properties of natural fibre fabric reinforced epoxy composites by alkali treatment. Journal of Reinforced Plastics and Composites, 31(6), 425-437. https://doi.org/10.1177/0731684412439494. 57. Prome, F. S., Hossain, M. F., Rana, M. S., Islam, M. M., & Ferdous, M. S. (2025). Different chemical treatments of natural fiber composites and their impact on water absorption behavior and mechanical strength. Hybrid Advances, 8, 100379. https:// doi.org/10.1016/j.hybadv.2025.100379. 58. Gassan, J., & Bledzki, A. K. (1999). Possibilities for improving the mechanical properties of jute/epoxy composites by alkali treatment of fibres. Composites Science and Technology, 59(9), 1303-1309. https://doi.org/10.1016/S0266-3538(98)00169-9. 59. Le Moigne, N., Longerey, M., Taulemesse, J.-M., Bénézet, J.-C., & Bergeret, A. (2014). Study of the interface in natural fibres reinforced poly(lactic acid) biocomposites modified by optimized organosilane treatments. Industrial Crops and Products, 52, 481-494. https://doi.org/10.1016/j.indcrop.2013.11.022. 60. Islam, T., Chaion, M. H., Jalil, M. A., Rafi, A. S., Mushtari, F., Dhar, A. K., & Hossain, S. (2024). Advancements and challenges in natural fiber-reinforced hybrid composites: A comprehensive review. SPE Polymers, 5(4), 481-506. https:// doi.org/10.1002/pls2.10145. 61. Lee, B.-H., Kim, H.-S., Lee, S., Kim, H.-J., & Dorgan, J. R. (2009). Bio-composites of kenaf fibers in polylactide: role of improved interfacial adhesion in the carding process. Composites Science and Technology, 69(15–16), 2573-2579. https://doi.org/10.1016/j.compscitech.2009.07.015. 62. Alix, S., Lebrun, L., Morvan, C., & Marais, S. (2011). Study of water behaviour of chemically treated flax fibresbased composites: A way to approach the hydric interface. Composites Science and Technology, 71(6), 893-899. https:// doi.org/10.1016/j.compscitech.2011.02.004. 63. Rauf, F., Umair, M., Shaker, K., Nawab, Y., Ullah, T., & Ahmad, S. (2023). Investigation of chemical treatments to enhance the mechanical properties of natural fiber composites. International Journal of Polymer Science, 4719481, 1-13. https://doi.org/10.1155/2023/4719481. 64. McKay, I., Vargas, J., Yang, L., & Felfel, R. M. (2024). A review of natural fibres and biopolymer composites: progress, 10/11
limitations, and enhancement strategies. Materials, 17(19), 4878. https://doi.org/10.3390/ma17194878. PMid:39410449. 65. Xie, Y., Hill, C. A. S., Xiao, Z., Militz, H., & Mai, C. (2010). Silane coupling agents used for natural fiber/polymer composites: A review. Composites. Part A, Applied Science and Manufacturing, 41(7), 806-819. https://doi.org/10.1016/j. compositesa.2010.03.005. 66. Bledzki, A. K., Reihmane, S., & Gassan, J. (1996). Properties and modification methods for vegetable fibers for natural fiber composites. Journal of Applied Polymer Science, 59(8), 1329-1336. https://doi.org/10.1002/(SICI)10974628(19960222)59:8<1329::AID-APP17>3.0.CO;2-0. 67. Owen, M. M., Ishiaku, U. S., Danladi, A., Dauda, B. M., & Romli, A. Z. (2018). Mechanical properties of epoxy-coated sodium hydroxide and silane treated kenaf/recycled polyethylene tereph-thalate (RPET) composites: effect of chemical treatment. AIP Conference Proceedings, 1985(1), 030001. https://doi. org/10.1063/1.5047159. 68. Rothenhäusler, F., Ouali, A.-A., Rinberg, R., Demleitner, M., Kroll, L., & Ruckdaeschel, H. (2024). Influence of sodium hydroxide, silane, and siloxane treatments on the moisture sensitivity and mechanical properties of flax fiber composites. Polymer Composites, 45(10), 8937-8948. https://doi.org/10.1002/ pc.28386. 69. John, K., & Naidu, S. V. (2004). Effect of fiber content and fiber treatment on flexural properties of sisal fiber/glass fiber hybrid composites. Journal of Reinforced Plastics and Composites, 23(15), 1601-1605. https://doi.org/10.1177/0731684404039799. 70. Zulyadain, Z., Yelwa, J. M., Abdullahi, S., Gwangwazo, I. U., & Ojo, O. (2024). Effect of benzoyl chloride and fiber loading on mechanical properties and biodegradation of poly lactic acid/sugarcane bagasse fibre composites. European Journal of Applied Science, Engineering and Technology, 1(1), 38-52. https://doi.org/10.59324/ejaset.2023.1(1).05. 71. Liao, Z., Hu, Y., Shen, Y., Chen, K., Qiu, C., Yang, J., & Yang, L. (2024). Investigation into the reinforcement modification of natural plant fibers and the sustainable development of thermoplastic natural plant fiber composites. Polymers, 16(24), 3568. https://doi.org/10.3390/polym16243568. PMid:39771421. 72. Jiyas, N., Sasidharan, I., Kumar, B. K., Gopakumar, B., & Dan, M. (2024). Harnessing the potential of Pseudoxytenanthera bamboo rhizome for enhanced high-friction assistive solutions. Journal of Cleaner Production, 451, 142114. https://doi. org/10.1016/j.jclepro.2024.142114. 73. Izwan, S. M., Sapuan, S. M., Zuhri, M. Y. M., & Mohamed, A. R. (2021). Thermal stability and dynamic mechanical analysis of benzoylation treated sugar palm/kenaf fiber reinforced polypropylene hybrid composites. Polymers, 13(17), 2961. https://doi.org/10.3390/polym13172961. PMid:34503001. 74. Dipta, M. S. I, Haque, S., Soshi, S. S., & Gafur, M. A. (2025). Statistical determination of mechanical strength of talipot palm fiber using Weibull distribution. Polymer Bulletin, 82(9), 3785-3804. https://doi.org/10.1007/s00289-025-05693-8. 75. Andersons, J., Spārniņš, E., & Joffe, R. (2006). Stiffness and strength of flax fiber/polymer matrix composites. Polymer Composites, 27(2), 221-229. https://doi.org/10.1002/pc.20184. 76. Mylsamy, B., Shanmugam, S. K. M., Aruchamy, K., Palanisamy, S., Nagarajan, R., & Ayrilmis, N. (2024). A review on natural fiber composites: polymer matrices, fiber surface treatments, fabrication methods, properties, and applications. Polymer Engineering and Science, 64(6), 2345-2373. https://doi. org/10.1002/pen.26713. 77. Ali, A., Islam, M. S., Hamdan, S., & Abdullah, M. (2025). Enhancing the performance of hybrid bio-composites reinforced with natural fibers by using coupling agents. Materials Research Polímeros, 36(2), e20260016, 2026
Recent advances in natural fiber treatments for enhanced composite performance Express, 12(3), 035504. https://doi.org/10.1088/2053-1591/ ad92f4. 78. Mutjé, P., Vallejos, M. E., Gironès, J., Vilaseca, F., López, A., López, J. P., & Méndez, J. A. (2006). Effect of maleated polypropylene as coupling agent for polypropylene composites reinforced with hemp strands. Journal of Applied Polymer Science, 102(1), 833-840. https://doi.org/10.1002/app.24315. 79. El-Sabbagh, A. (2014). Effect of coupling agent on natural fibre in natural fibre/polypropylene composites on mechanical and thermal behaviour. Composites. Part B, Engineering, 57, 126-135. https://doi.org/10.1016/j.compositesb.2013.09.047. 80. George, M., Mussone, P. G., & Bressler, D. C. (2014). Surface and thermal characterization of natural fibres treated with enzymes. Industrial Crops and Products, 53, 365-373. https:// doi.org/10.1016/j.indcrop.2013.12.037. 81. Karaduman, Y., Gokcan, D., & Onal, L. (2013). Effect of enzymatic pretreatment on the mechanical properties of jute fiber-reinforced polyester composites. Journal of Composite Materials, 47(10), 1293-1302. https://doi.org/10.1177/0021998312446826. 82. Vigneswaran, C., & Jayapriya, J. (2010). Effect on physical characteristics of jute fibres with cellulase and specific mixed enzyme systems. Journal of the Textile Institute, 101(6), 506513. https://doi.org/10.1080/00405000802542333. 83. Zwane, P. E., Ndlovu, T., Mkhonta, T. T., Masarirambi, M. T., & Thwala, J. M. (2019). Effects of enzymatic treatment of sisal fibres on tensile strength and morphology. Scientific African, 6, e00136. https://doi.org/10.1016/j.sciaf.2019.e00136. 84. Shahzad, A., Tanasa, F., & Teaca, C. A. (2022). Surface treatment methods of natural fibres and their effects on biocomposites. Sawston: Woodhead Publishing. https://doi.org/10.1016/ C2019-0-04389-0. 85. Mahmud, S. H., Das, S. C., Saha, A., Islam, T., Paul, D., Akram, M. W., Jahan, M. S., Mollah, M. Z. I., Gafur, M. A., & Khan, R. A. (2025). Next Sustainability Effect of glass fiber hybridization and radiation treatment to improve the performance of sustainable natural fiber-based hybrid (jute / glass) composites. Next Sustainability, 6, 100104. https://doi. org/10.1016/j.nxsust.2025.100104. 86. Belgacem, M. N., Bataille, P., & Sapieha, S. (1994). Effect of corona modification on the mechanical properties of polypropylene/cellulose composites. Journal of Applied Polymer Science, 53(4), 379-385. https://doi.org/10.1002/ app.1994.070530401. 87. Izdebska-Podsiadły, J. (2019). Application of plasma in printed surfaces and print quality. In S. Thomas, M. Mozetič, U. Cvelbar, P. Špatenka, & K.M. Praveen (Eds.), Non-thermal plasma technology for polymeric materials: applications in composites, nanostructured materials, and biomedical fields (pp. 159-191). Amsterdam: Elsevier. https://doi.org/10.1016/ B978-0-12-813152-7.00006-8. 88. Mesquita, R. G. A., César, A. A. S., Mendes, R. F., Mendes, L. M., Marconcini, J. M., Glenn, G., & Tonoli, G. H. D. (2017).
Polímeros, 36(2), e20260016, 2026
Polyester composites reinforced with corona-treated fibers from pine, eucalyptus and sugarcane bagasse. Journal of Polymers and the Environment, 25(3), 800-811. https://doi.org/10.1007/ s10924-016-0864-6. 89. Gassan, J., & Gutowski, V. S. (2000). Effects of corona discharge and UV treatment on the properties of jute-fibre expoxy composites. Composites Science and Technology, 60(15), 2857-2863. https://doi.org/10.1016/S0266-3538(00)00168-8. 90. Campomori, J. B., Hugen, L. N., Silva, F. A., Toledo Filho, R. D., Guimarães, T. C., Bufalino, L., Sanadi, A. R., Barsberg, S., Ferreira, S. R., & Tonoli, G. H. D. (2024). Effect of hot water and corona discharge treatments on the bonding behavior of jute fibers in polyester matrix. Discover Materials, 4(1), 14. https://doi.org/10.1007/s43939-024-00085-7. 91. Ghalme, S., Hayat, M., & Harne, M. (2024). A comprehensive review of natural fibers : bio-based constituents for advancing sustainable materials technology. Journal of Renewable Materials, 13(2), 273-295. https://doi.org/10.32604/jrm.2024.056275. 92. Sun, D. (2016). Surface modification of natural fibers using plasma treatment. In D. Sun (Ed.), Biodegradable green composites (pp. 18-39). Hoboken: John Wiley & Sons. https:// doi.org/10.1002/9781118911068.ch2. 93. Gupta, U. S., Dhamarikar, M., Dharkar, A., Chaturvedi, S., Kumrawat, A., Giri, N., Tiwari, S., & Namdeo, R. (2020). Plasma modification of natural fiber: A review. Materials Today: Proceedings, 43(Part 1), 451-457. https://doi.org/10.1016/j. matpr.2020.11.973. 94. Morent, R., De Geyter, N., Verschuren, J., De Clerck, K., Kiekens, P., & Leys, C. (2008). Non-thermal plasma treatment of textiles. Surface and Coatings Technology, 202(14), 34273449. https://doi.org/10.1016/j.surfcoat.2007.12.027. 95. Carneiro, N., Souto, A. P., Silva, E., Marimba, A., Tena, B., Ferreira, H., & Magalhaes, V. (2001). Dyeability of corona‐ treated fabrics. Coloration Technology, 117(5), 298-302. https:// doi.org/10.1111/j.1478-4408.2001.tb00079.x. 96. Mukhopadhyay, S., & Fangueiro, R. (2009). Physical modification of natural fibers and thermoplastic films for composites: a review. Journal of Thermoplastic Composite Materials, 22(2), 135-162. https://doi.org/10.1177/0892705708091860. 97. Bozaci, E., Sever, K., Sarikanat, M., Seki, Y., Demir, A., Ozdogan, E., & Tavman, I. (2013). Effects of the atmospheric plasma treatments on surface and mechanical properties of flax fiber and adhesion between fiber-matrix for composite materials. Composites. Part B, Engineering, 45(1), 565-572. https://doi.org/10.1016/j.compositesb.2012.09.042. Received: Oct. 19, 2025 Revised: Jan. 02, 2026 Accepted: Jan. 06, 2026 Editor-in-Chief: Sebastião V. Canevarolo
11/11
ISSN 1678-5169 (Online)
https://doi.org/10.1590/0104-1428.20250066
Application of biopolymers in hydrogels for tissue repair with bioextracts: systematic review Otávio Soares Nascimento1 , Adriano Freitas de Santana2 , Cláudia Sampaio de Andrade Lima3 , Ana Cristina Silveira Martins1* and Ricardo Yara1 Departamento de Engenharia Biomédica, Universidade Federal de Pernambuco – UFPE, Recife, PE, Brasil 2 Instituto Keizo Asami – iLIKA, Universidade Federal de Pernambuco – UFPE, Recife, PE, Brasil 3 Departamento de Biofísica e Radiobiologia, Universidade Federal de Pernambuco – UFPE, Recife, PE, Brasil 1
*martinsanaacs@gmail.com
Abstract Biomaterials engineering has evolved rapidly, with a particular emphasis on biofunctionalized hydrogels for tissue repair. This systematic review, based on PRISMA 2020 guidelines, analyzed 75 studies from the SCOPUS database, evaluating biopolymers combined with bioextracts for wound healing. Bibliometric analysis revealed a significant increase in publications from 2022 onward, with a focus on Biomaterials Engineering and Biotechnology. The most productive centers were the departments of Medical Nanotechnology, Biotechnology, and Biomedical Engineering. Among the central authors, Li, Doostan, and Karamanlioglu stood out. The most cited articles focused on antimicrobial and regenerative strategies. China leads in scientific production, followed by India and the USA. The most frequent keywords included “wound healing,” “hydrogel,” and “biocompatibility.” In vitro studies (53%) and combined in vitro/ in vivo studies (43%) predominated. It is concluded that biofunctionalized hydrogels hold high therapeutic potential but require methodological standardization and clinical validation for safe application in regenerative medicine. Keywords: biopolymers, controlled drug release, plant extracts, healing, regenerative medicine. Data Availability: All data supporting the findings of this study are included in this article and its supplementary materials. How to cite: Nascimento, O. S., Santana, A. F., Lima, C. S. A., Martins, A. C. S., & Yara, R. (2026). Application of biopolymers in hydrogels for tissue repair with bioextracts: systematic review. Polímeros: Ciência e Tecnologia, 36(2), e20260019. https://doi.org/10.1590/0104-1428.20250066
1. Introduction In recent decades, advances in biomaterials engineering have been transforming the landscape of regenerative medicine, offering innovative solutions for tissue repair[1]. Among these technologies, hydrogels stand out due to their ability to mimic the extracellular matrix (ECM), facilitating cell adhesion and proliferation, angiogenesis, and the controlled release of bioactive compounds[2]. According to Xu[3] and Pankoh et al.[4], the incorporation of natural biopolymers such as chitosan, alginate, collagen, and silk fibroin endows these materials with essential characteristics, including biocompatibility, biodegradability, antimicrobial capacity, and tunable mechanical properties. The functionalization of hydrogels with plant bioextracts has become a promising strategy to enhance therapeutic properties such as anti-inflammatory, antioxidant, and regenerative activities. The incorporation of Amaranthus spinosus extracts into chitosan-based biopatches has shown the ability to stimulate tissue regeneration, modulate inflammatory responses, and inhibit bacterial infections. These systems act as a protective barrier over the wound, fostering the formation of a microenvironment conducive to healing and functional tissue recovery[5].
Polímeros, 36(2), e20260019, 2026
Furthermore, advances in materials engineering have enabled the combination of hydrogels with antimicrobial peptides (AMPs), such as P9-4 (a peptide), which are effective against multidrug-resistant pathogens like MRSA (methicillin-resistant Staphylococcus aureus) and Pseudomonas aeruginosa. When conjugated to the GelMa (methacrylated gelatin) hydrogel matrix, these peptides promote localized and effective antimicrobial activity, with low toxicity and high selectivity, overcoming one of the main limitations of conventional hydrogels: the lack of intrinsic antimicrobial properties[6]. According to Jing et al.[7] and Korzeniewska et al.[8], these approaches reflect a growing trend toward combining the structural properties of hydrogels with the therapeutic functionalities of bioactive compounds, whether natural or synthetic, to achieve a multifunctional approach to tissue regeneration. This perspective has been reinforced by the use of emerging technologies such as plasma activation, peptide conjugation, and solvent molding, which significantly expand the therapeutic potential of these biomaterials. However, despite continuous advances in functionalized hydrogel research, significant gaps remain regarding the consolidation of robust scientific evidence related to their efficacy, safety, and physicochemical characterization in clinical settings.
1/14
R R R R R R R R R R R R R R
Nascimento, O. S., Santana, A. F., Lima, C. S. A., Martins, A. C. S., & Yara, R. Given the growing interest in the use of biopolymer-based hydrogels functionalized with bioactive compounds, especially plant bioextracts, as promising strategies for tissue repair, a significant gap persists in the consolidation of scientific knowledge regarding their efficacy, safety, and clinical feasibility[9,10]. Although preclinical studies report relevant therapeutic properties such as anti-inflammatory, antimicrobial, and regenerative effects[11,12], there remains considerable methodological heterogeneity among published trials, which hinders the generalization of results and the formulation of evidence-based recommendations. Therefore, this study aimed to conduct a systematic review on the application of biopolymers incorporated into hydrogels containing bioextracts for tissue repair, with emphasis on evaluating the therapeutic efficacy, physicochemical properties of these systems, and their potential applications in clinical contexts.
2. Materials and Methods The entire methodological process was conducted in accordance with the PRISMA 2020 (Preferred Reporting Items for Systematic Reviews and Meta-Analyses) guidelines, ensuring transparency, reproducibility, and methodological rigor throughout the stages of this study.
Sampaio and Mancini[13] highlight systematic review as a critical appraisal strategy that uses literary sources as an effective form of intervention to clarify a body of information on a specific topic. Berwanger et al.[14] emphasize how to conduct systematic reviews and further underscore the importance of this type of research for scientific networks, particularly in the field of health. Following the PRISMA 2020 guidelines, it was possible to analyze the studies systematically using four steps: (1) identification; (2) screening; (3) eligibility; and (4) inclusion, as illustrated in Figure 1, described in detail in items 2.1, 2.2, 2.3, and 2.4. Initially, one thousand one hundred and twenty-two articles were identified in the SCOPUS ELSEVIER database. After applying the filters, nine hundred and sixty-one articles were excluded for not meeting the basic research criteria, as the title, abstract and/or objectives were not compatible with the scope of the study, resulting in one hundred and sixty-one studies for more detailed screening. Of these, fortytwo were eliminated for not meeting the inclusion criteria, totaling one hundred and nineteen studies that advanced to methodological evaluation. During this preliminary assessment, nine studies were excluded, leaving one hundred and ten articles whose full texts were analyzed for eligibility.
Figure 1. PRISMA flow diagram illustrating the phases of identification, screening, eligibility assessment, and inclusion of studies in the systematic review, highlighting the database used and the reasons for exclusions. 2/14
Polímeros, 36(2), e20260019, 2026
Application of biopolymers in hydrogels for tissue repair with bioextracts: systematic review Among these, thirty-five were excluded for various reasons: twenty-two were not aligned with the research question, seven lacked relevant data, five did not meet the inclusion criteria, and one studie presented a conflict of interest. In the end, seventy-five articles were selected to compose the systematic review, representing the set of publications that met the selection and analysis criteria defined in the protocol. Each filter will be detailed in the following paragraphs. This rigorous process, represented by the PRISMA 2020 flow diagram, ensures the transparency and reproducibility of the research.
2.1 Identification For the identification of studies, the search was conducted in the SCOPUS database, selected for its broad coverage of scientific journals and its indexing of high-impact publications in the fields of Biotechnology, Biomaterials Engineering, and Regenerative Medicine. Additionally, Scopus includes records from internationally recognized databases such as PubMed, Medline, and Embase[15]. To guide the search and ensure the selection of studies aligned with the objectives of the review, a strategy combining controlled vocabulary terms with Boolean operators was employed, allowing for greater precision in data retrieval. Several search terms were used: “Biopolymers” AND “Hydrogel” AND “Tissue repair” AND “lipid system.” The term “lipid system” was entered once; these hydrogels are designed for use in lipid complexes to repair the skin barrier. This initial search resulted in the identification of 1,122 publications. After filtering, the number was reduced to 161 articles, which underwent subsequent stages of screening and careful selection, with the aim of including only studies with methodological rigor and thematic relevance to the scope of the review. This is because the initial search is intentionally broad, and in the following stages, the application of strict eligibility criteria removes duplicates and studies outside the scope, ensuring that only relevant and comparable evidence is included in the final synthesis. Thus, the filters used in this review were: articles in English, within the time frame of 2014 to 2024, and original articles.
2.2 Screening The screening stage aimed to refine the selection of the initially identified studies by excluding those that did not meet the defined methodological and thematic criteria, ensuring that only the most relevant publications for the purposes of the research would proceed to the next phases. This process was conducted in two complementary stages. In the first stage, articles from literature reviews, narratives, scope reviews, or critiques were removed from the 161 studies initially identified. This initial filtering allowed the focus to remain exclusively on original studies with primary data, ensuring greater consistency in the analysis. In the second stage, the remaining 119 studies underwent thorough screening based on the reading of titles and abstracts, performed independently by two reviewers. Studies were excluded at this stage if: they did not directly address the application of biopolymers in hydrogels for tissue repair; they involved populations or models incompatible with the objectives of the review, studies only with microorganisms or Polímeros, 36(2), e20260019, 2026
cell lines, models without healing or regeneration outcomes, or populations outside the defined scope; or did not present a clear methodology for evaluating the effects related to tissue bioengineering or the use of lipid systems and bioextracts. Following this screening, 9 studies were excluded, leaving 110 articles considered eligible for full-text reading and in-depth evaluation.
2.3 Eligibility The eligibility stage consisted of a full-text review of the 110 previously selected studies, with the goal of ensuring that only those with methodological rigor and direct relevance to the review objectives were included in the final analysis. To maintain consistency in the selection process, the inclusion criteria were defined in advance. Eligible studies were original research articles that clearly and directly addressed the application of biopolymers incorporated into hydrogels with a focus on tissue repair, particularly those that employed bioextracts as bioactive agents in the regenerative process, within the time frame of 2014 to 2024. During this stage, 35 studies were excluded because they did not meet the established methodological criteria. The main reasons for exclusion included: misalignment with the scope of the research question, lack of relevant data for the proposed analysis, failure to meet the predefined inclusion criteria, and identification of a conflict of interest that compromised the impartiality of the results.
2.4 Inclusion and data extraction After completing the identification, screening, and eligibility stages, 75 studies were selected for the final analysis. Data extraction followed a standardized protocol, ensuring consistency and comparability across the collected information. Among the extracted data were complete bibliographic details such as author names, study title, year of publication, scientific journal, institutional affiliation, citation count, keywords, and the main findings related to the investigated topic. To enhance understanding of the scientific output on the subject, a complementary bibliometric analysis was conducted using the VOSviewer software (version 1.6.20). This tool enabled the mapping of collaboration networks among researchers and institutions, the identification of keyword co-occurrence patterns, and the observation of the temporal evolution of publications. The use of VOSviewer provided a deeper insight into the core themes of the literature and the structural connections within the field. Data extraction and analysis were conducted independently by two reviewers to minimize bias and increase the reliability of the results. A third reviewer verified the entire process, ensuring the validation of the collected information and the consistency of the bibliometric analyses, thereby contributing to the methodological rigor of the review.
2.5 Data synthesis and analysis The synthesis of data included in the systematic review was carried out through an integrated approach, combining qualitative and quantitative methods to ensure a more in-depth and comprehensive analysis of the available scientific literature on the topic. 3/14
Nascimento, O. S., Santana, A. F., Lima, C. S. A., Martins, A. C. S., & Yara, R. Initially, a descriptive analysis was conducted to examine the methodological characteristics of the selected studies, with emphasis on the strategies adopted, experimental designs employed, and main limitations reported. This step allowed for an understanding of the predominant methodological profile and the evaluation of the robustness of the available data. Subsequently, the findings were thematically organized, grouping the studies into specific analytical categories, such as: biomedical applications of biopolymers in regenerative processes; therapeutic potential of hydrogels functionalized with bioextracts; and interactions between lipid systems and polymeric materials in the context of tissue healing. This categorization facilitated the identification of conceptual patterns and the coherent structuring of data in line with the objectives of the review. Additionally, whenever the data allowed for statistical compatibility, quantitative techniques were used, including descriptive analyses and, when applicable, meta-analysis, to quantify the impact and efficacy of biopolymers employed in tissue repair strategies. The adoption of this mixed methodological approach helped to uncover prevailing trends, highlight relevant connections among the addressed themes, and identify gaps in the literature. This made it possible to suggest strategic directions for future investigations in the field of biotechnology applied to biomaterials engineering and regenerative medicine. As part of the characterization of the included body of literature, a bibliometric analysis focusing on the geographical distribution of publications was conducted. For this purpose, the full counting method was used, in which each country listed in the institutional affiliations of the articles receives full credit for the publication, regardless of the number of coauthoring countries. Thus, in articles with multiple international affiliations, all participating countries are fully counted, without proportional weighting. This approach allows for the identification of the presence and overall contribution of each country within the set of included studies, favoring more inclusive analyses of scientific collaborations. Unlike fractional counting, which distributes credit proportionally among the participating countries or institutions, full counting preserves the totality of participations, enhancing the visibility of national contributions in multinational contexts. Prior to the qualitative analysis, the included studies were systematically organized into five central thematic categories, aiming to facilitate the interpretation of results, identify recurring patterns, and highlight gaps and trends in scientific production. The definition of these categories followed an integrated methodological approach composed of three stages: the first consisted of an exploratory reading of the abstracts and keywords of the 75 selected articles; the second involved a qualitative analysis with thematic coding, based on the identification of recurring patterns in the topics addressed, according to the method proposed by Braun and Clarke[16]; and the third stage employed a co-occurrence analysis of terms using the VOSviewer software (version 1.6.20), as recommended by Saiz-Alvarez[17], allowing for the 4/14
visualization of thematic clusters and conceptual nuclei present in the literature. The triangulation of qualitative and bibliometric approaches, as proposed by Donthu et al.[18], enabled the identification of five main thematic areas for classifying the analyzed studies: (1) biomaterials engineering; (2) biotechnology; (3) pharmaceutics and pharmaceutical technology; (4) polymer chemistry; and (5) regenerative medicine. The classification of studies into these areas was conducted independently by two reviewers, and any disagreements were resolved by consensus, with final validation performed by a third reviewer, ensuring greater methodological rigor and minimizing potential bias. During this analysis, the VOSviewer software was used to map citations among the documents included in the systematic review, using direct citation as the type of analysis and the documents themselves as the units of analysis. Each node represents a study included in the systematic review, with node size proportional to the number of citations received. Colors indicate the distribution of documents across different thematic clusters.
3. Results and Discussions 3.1 Temporal analysis Based on the data obtained through the systematic review process, it was possible to construct a timeline of publications related to the topic of biopolymers combined with bioextracts applied to wound treatment. According to Figure 2, a progressive increase in research on the topic was observed over the years. Between 2014 and 2021, the number of publications fluctuated irregularly, with some years showing no records (2014, 2016, and 2018) and a peak in 2020, with four publications. In 2022, there was a significant increase of 600% in the number of publications compared to the previous year, totaling 18 publications indexed in the SCOPUS database. This growth intensified in 2024, which recorded the highest number of publications to date, with 26 entries, highlighting the growing scientific interest in the field. The evolution of scientific publications on the use of biopolymers in hydrogels for tissue repair highlights a field in continuous expansion, driven by technological advances and transformations in the global scientific landscape. Between 2014 and 2018, the number of published studies remained limited, which may be attributed to initial methodological challenges, the need for validation of new biomaterials, and possible funding constraints in translational research. From 2020 onward, there has been an increase in publications, indicating growing interest from the scientific community and showing exponential growth. This growth intensified particularly from 2022, reflecting the consolidation of innovative techniques, encouragement of research in tissue engineering, and the strengthening of policies supporting regenerative biotechnology, such as the consolidation of electroconductive hydrogels, the conjugation of antimicrobial peptides, plasma activation, the “green” synthesis of chitosan, and responsive dressings. Polímeros, 36(2), e20260019, 2026
Application of biopolymers in hydrogels for tissue repair with bioextracts: systematic review
Figure 2. Temporal distribution of articles between 2014 and 2024.
The development of new technologies, such as green synthesis of nanoparticles, combined with the improvement of in vivo preclinical models, has propelled the application of functionalized hydrogels in regenerative therapies. Additionally, the COVID-19 pandemic underscored the urgent need for innovative biomedical solutions, redirecting investments toward research in tissue repair. This temporal analysis not only demonstrates the maturation of the field but also highlights opportunities for more integrated and translational investigations. The recent growth reflects both technical advances and clinical demands, suggesting a promising future for the practical application of these biomaterials. However, it is essential to ensure that the increased volume of publications translates into effective therapeutic innovations, with international collaborations and sustained investments serving as catalysts for this progress.
3.2 Thematic analysis of publications In the radar chart (Figure 3), the distribution of the analyzed articles can be observed according to five areas of study: Biomaterials Engineering, Biotechnology, Pharmaceutics and Pharmaceutical Technology, Polymer Chemistry, and Regenerative Medicine. For the thematic analysis, studies were categorized based on the predominant focus of each article, central objective, and main outcomes. This thematic distribution analysis revealed a higher concentration of publications in the field of Biomaterials Engineering, followed by Biotechnology and Pharmaceutics and Pharmaceutical Technology. In contrast, Regenerative Medicine and Polymer Chemistry showed lower representation, indicating a scientific focus predominantly directed toward the development of new biomaterials and biotechnological applications for wound treatment. Polímeros, 36(2), e20260019, 2026
The fields of Biotechnology and Pharmaceutics confirm the trend of functionalizing biomaterials with bioextracts and controlled release systems, as evidenced in the studies by Shehabeldine et al.[19] and Khoshnevisan et al.[20]. In the study by Shehabeldine et al.[19], silver nanoparticles stabilized with chitosan (Chi/Ag-NPs) were developed using an environmentally friendly method, highlighting the functionalization of chitosan with antimicrobial, antioxidant, and wound-healing properties, as well as the controlled release of silver ions. Khoshnevisan et al.[20] demonstrated the use of cellulose acetate/polycaprolactone (CA/PCL) nanofibers impregnated with propolis, resulting in biomaterials with high antimicrobial and antioxidant capacities, functionalized for the gradual release of the bioextract. These advances exemplify the potential of biopolymers as carriers for bioextracts in biomedical and pharmaceutical applications, promoting specific therapeutic properties and optimizing the performance of controlled drug delivery systems. In contrast, the reduced representation of Polymer Chemistry (3%) and Regenerative Medicine (6%) reveals significant gaps. While technological development advances, challenges remain in understanding the molecular mechanisms and translating these materials into clinical practice. This asymmetric distribution suggests that the field prioritizes applied solutions aligned with translational medicine demands but still lacks integration between fundamental and applied research. The future challenge lies in finding a balance by fostering collaborations that link material development with investigations into the principles of tissue regeneration and optimization of the molecular properties of polymers. Thematically, studies have evolved from traditional approaches using natural polymers, such as chitosan and alginate, to more complex strategies, including electroconductive hydrogels[21] and smart systems for diabetic wound care. 5/14
Nascimento, O. S., Santana, A. F., Lima, C. S. A., Martins, A. C. S., & Yara, R.
Figure 3. Radar chart showing the classification of articles distributed across five central themes.
Figure 4. Departments with the highest number of publications. Generated using VOSviewer software
This progression is consistent with the predominance of publications in Biomaterials Engineering and Biotechnology (Figure 3), while areas such as Regenerative Medicine and Polymer Chemistry showed lower representation, an opportunity to be explored in future research.
3.3 Institutional analysis: central departments and interdisciplinary collaborations Through the research process, a total of 245 departments were identified as part of the most cited departmental network, organized into 31 clusters, highlighting a remarkably structured configuration of research on biopolymers and bioextracts for 6/14
tissue repair. The network visualization analysis (Figure 4) demonstrates the formation of department groupings with strong internal collaboration. These departments exhibited the highest number of connections and strong link strength, positioning themselves centrally within the structure, which indicates their high relevance and influence in research on biopolymers combined with bioextracts for wound treatment. The identification of 245 departments distributed across 31 specialized clusters reflects a mature research field, with well defined patterns of specialization and interinstitutional collaboration. The existence of multiple clusters also suggests a diversity of approaches and the integration of different areas of knowledge. Polímeros, 36(2), e20260019, 2026
Application of biopolymers in hydrogels for tissue repair with bioextracts: systematic review In this type of analysis, Total Link Strength (TLS) quantifies the intensity of bibliographic links between authors, highlighting how close they are in terms of subject matter. The network is formed by three key institutions: the Department of Medical Nanotechnology (Total Link Strength 731), Higher Institute of Biotechnology (Total Link Strength 574), and Department of Biomedical Engineering (Total Link Strength 504). Together, these centers constitute a strategic axis responsible for approximately 68% of high-impact publications in the field, highlighting how the integration of medical nanotechnology, biotechnology, and biomedical engineering has served as a driving force for major advances in the area. A deeper analysis of collaborative dynamics revealed three distinct patterns of scientific interaction. The first involves strong integration among the leading institutional centers, characterized by frequent co-authorships and shared use of technological resources. Secondly, highly specialized thematic networks stand out, responsible for around 82% of the methodological innovations identified. Lastly, emerging connections with peripheral institutions have been progressively contributing to expanding the scope and diversity of scientific production in the field. These findings not only confirm previous studies on innovation networks in biomaterials but also offer new perspectives on how strategic positioning within a network directly influences scientific productivity. Central departments act as true knowledge dissemination hubs, facilitating the flow of information between different specialties and promoting interdisciplinary integration[22]. From the analysis, four particularly relevant strategic opportunities emerge: (1) the potential of the interface between nanotechnology and bioengineering to develop smart delivery systems; (2) the possibility of accelerating clinical translation through the expansion of validation networks; (3) promising applications of artificial intelligence in the design of biomaterials; and (4) the optimization of data sharing through collaborative platforms.
These results have significant implications for science policy, suggesting the need for targeted investments in shared infrastructure and mobility programs among leading centers of excellence. Compared to other fields in biomedicine, this analysis reveals an exceptional degree of interconnection, likely reflecting the inherently interdisciplinary nature of research on biopolymers. This characteristic is evident in the integration of knowledge from nanotechnology, biomedical engineering, pharmaceutics, and biotechnology, as emphasized by Cavalcante et al.[1] and Augustine et al. [23] , who highlight the importance of these convergences for advancing innovative therapeutic technologies. However, the concentration of connections within a few central clusters, as evidenced by the departments with the Polímeros, 36(2), e20260019, 2026
highest link strength (Higher Institute of Biotechnology, Department of Medical Nanotechnology, and Department of Biomedical Engineering), may pose a risk of fragility in the scientific network. According to Binsfeld[24] and Pereira et al.[25], limiting collaborations to a few cores may restrict the diversity of approaches and hinder effective knowledge transfer to peripheral or emerging institutions. Therefore, funding policies that prioritize not only major centers but also the training of new institutional actors and the creation of more inclusive collaborative networks are essential to ensure the sustainable advancement of the field. Moreover, interdisciplinarity requires continuous integration of knowledge, from basic science to clinical application, as emphasized by Bodla et al.[2] and Çelebi et al. [6] . This integration is crucial to overcoming methodological and regulatory challenges and ensuring that scientific advances are translated into effective therapeutic solutions. The COVID-19 pandemic highlighted the urgency of accelerating this process, as demonstrated by the studies of Hu et al.[21] and Khoshnevisan et al.[20], which underscore the role of innovative biomaterials with antimicrobial and regenerative properties. Therefore, strengthening international collaborations, investing in advanced infrastructure, and promoting inclusive and sustainable policies are essential for consolidating functionalized biopolymer research as one of the pillars of modern biomedicine.
3.4 Bibliographic coupling analysis in scientific productions Based on the bibliographic coupling analysis among authors (Figure 5), it was possible to identify the formation of different clusters, representing groups of researchers who share common references in their scientific output. Total Link Strength (TLS) is also used, which indicates the strength of bibliographic connections between authors, reflecting the degree of thematic proximity between them. Authors with high TLS values share a large number of references with other researchers, indicating alignment in their research areas. The central “nodes” identified include the authors Li, Suming (Cluster 3, Total Link Strength: 1926, Links: 3), Doostan, Maryam (Cluster 1, Total Link Strength: 746, Links: 115), and Karamanlioglu, Mehlika (Cluster 35, Total Link Strength: 269, Links: 39). Li, Suming’s high Total Link Strength, despite a small number of connections, suggests strong thematic specialization and a high degree of shared references with a few, yet highly relevant, authors. In contrast, Doostan, Maryam exhibits a large number of connections, indicating broader and more transversal engagement across different subgroups of the network. Karamanlioglu, Mehlika also demonstrates significant interaction within her cluster. The strength of these connections reflects thematic alignment and shared use of methodological frameworks[25]. These results reveal the existence of consolidated cores of scientific production, indicating closely related research lines and potential future collaborations within the field analyzed.
3.5 Document co-citation analysis The visualization generated, as illustrated in Figure 6, made it possible to identify the studies with the greatest impact in terms of the number of citations received, represented 7/14
Nascimento, O. S., Santana, A. F., Lima, C. S. A., Martins, A. C. S., & Yara, R. by larger nodes in the graph. Among the highlights, the study by Hu et al.[21] recorded 125 citations and was placed in Cluster 7; Khoshnevisan et al.[20] had 108 citations in Cluster 53;
Üstündağ Okur et al.[26] registered 104 citations in Cluster 50; Shehabeldine et al.[19] received 101 citations in Cluster 59; and Sonamuthu et al.[27] totaled 100 citations in Cluster 47.
Figure 5. Group of authors using similar bibliographic sources. Generated using VOSviewer software.
Figure 6. Co-citation map among documents generated using VOSviewer software. 8/14
Polímeros, 36(2), e20260019, 2026
Application of biopolymers in hydrogels for tissue repair with bioextracts: systematic review It was noted, however, that no direct links between the documents were identified, indicating the absence of cross-citations among them. This dispersion suggests that although these studies are highly cited, they belong to distinct or still unconnected research lines, reinforcing the thematic diversity found in the analyzed sample. Although the generated graph did not reveal explicit connections between the documents - meaning the most cited articles do not cite each other within the analyzed database, this did not hinder an interpretive reading based on the qualitative analysis of the texts. Through full-text reading of the most cited articles and inspection of their reference lists, it was possible to identify conceptual overlaps, methodological affinities, and converging application areas. Based on this approach, two distinct conceptual clusters emerged from the analyzed documents. The first cluster consists of the studies by Üstündağ Okur et al.[26], Khoshnevisan et al.[20], and Shehabeldine et al.[19], which share a focus on the development of biomaterials applied to wound healing. Common elements include the use of natural polymers (such as chitosan, alginate, and CA/PCL), the application of technologies like electrospinning, and the incorporation of bioactive compounds such as propolis and silver nanoparticles. While these articles do not directly cite one another, a strong methodological convergence is observed, including antimicrobial assays, topical formulations, and wound dressing engineering strategies, indicating a significant thematic affinity.
The second conceptual cluster involves the studies by Hu et al.[21] and Sonamuthu et al.[27], both centered on regenerative bioengineering approaches. These authors investigate the development of bioactive hydrogels and therapeutic strategies focused on cellular modulation, such as calcium ion-mediated signaling and inhibition of matrix metalloproteinase-9 (MMP-9). Their methodologies combine in vitro and in vivo assays applied to bone regeneration or diabetic wound healing, demonstrating strong alignment in terms of scope and scientific foundation. However, the absence of cross-citations among the most cited studies points to a dispersion of research lines, which may limit the construction of a common theoretical framework and the establishment of standardized methodological protocols[28]. Thus, even in the absence of explicit citation links between the most cited documents, the data suggest the existence of two major prevailing thematic axes: one focused on innovation in bioactive dressings and antimicrobial systems, and the other on tissue engineering with an emphasis on cellular modulation and functional regeneration. This qualitative interpretation complements the quantitative findings from the direct citation analysis, contributing to a deeper understanding of the theoretical-methodological structure of the mapped scientific literature. As shown in Table 1, the authors, article titles, abstracts, methodologies and keywords of the most cited articles are listed.
Table 1. Most cited articles in the analysis: Main articles identified through the analysis of direct citations in the VOSviewer software, based on the number of co-citations received. Author Hu et al.[21]
Khoshnevisan et al.[20]
Üstündağ Okur et al.[26]
Shehabeldine et al.[19]
Sonamuthu et al.[27]
Article title Piezoresistive MXene/Silk fibroin nanocomposite hydrogel for accelerating bone regeneration by Re-establishing electrical microenvironment Antibacterial and antioxidant assessment of cellulose acetate/ polycaprolactone nanofibrous mats impregnated with própolis An alternative approach to wound healing field; new composite films from natural polymers for mupirocin dermal delivery Multifunctional Silver Nanoparticles Based on Chitosan: Antibacterial, Antibiofilm, Antifungal, Antioxidant, and WoundHealing Activities MMP-9 responsive dipeptide-tempted natural protein hydrogel-based wound dressings for accelerated healing action of infected diabetic wound
Polímeros, 36(2), e20260019, 2026
Summary Tissue engineering, electrical stimulation, cell signaling (Ca2+/CALM), electrical microenvironment in bone
Methodology Experimental in vitro and in vivo
Keywords Bone regeneration, Electrical microenvironment, MXene, Hydrogel
Biomaterials and nanotechnology applied to healing, therapeutic use of propolis, electrospinning
Experimental (Synthesis and characterization)
Nanofibrous mats, Propolis, Electrospinning, Wound healing
Natural polymeric hydrogels (chitosan, alginate), controlled drug release, topical use of antibiotics Green synthesis of metal nanoparticles, chitosan as an antimicrobial and reducing agent, nanobiotechnology
Experimental study (in vitro Chitosan, Sodium alginate, and in vivo) Wound healing, Mupirocin
Experimental (Synthesis and bioassays)
Chitosan, Silver nanoparticles, Wound healing, Antimicrobial
MMP-9 (matrix metalloproteinase 9) in healing, therapeutic use of L-carnosine and curcumin, tissue bioengineering
Experimental (In vivo with diabetic mice)
Silk protein, Diabetic wound, MMP-9, Curcumin, L-carnosine
9/14
Nascimento, O. S., Santana, A. F., Lima, C. S. A., Martins, A. C. S., & Yara, R. As shown in Table 1, the most cited articles in the analysis were identified from the analysis of direct citations in the VOSviewer software, considering the number of co-citations received. It can be observed that these studies are mostly experimental and focus on the development of polymeric biomaterials and nanocomposites applied to tissue regeneration and healing, including hydrogel for bone regeneration, cellulose acetate/PCL nanofiber mats with propolis, natural composite films for mupirocin release, chitosan-based silver nanoparticles with antimicrobial activity, and MMP9-responsive hydrogel for diabetic wounds, indicating a core of highly co-cited literature for integrating bioactive properties and tissue engineering strategies.
3.6 Bibliographic coupling analysis between countries Figure 7 illustrates these relationships, where the size of the nodes represents the number of documents per country, and the thickness of the lines reflects the intensity of bibliographic connections. The colors are automatically assigned to clusters detected by the VOSviewer algorithm. This visualization provides a clear perspective of the organization, density, and interconnectivity of international bibliographic relations within the analyzed body of studies. It is worth noting that link strength is an indicator of thematic similarity between countries, not the number of citations received. Therefore, it serves as an effective parameter to understand the relative positioning and alignment of countries within the global network of scientific production. The data obtained allowed for the identification of interrelations between the scientific output of different countries, based on the shared bibliographic references among
the articles included in the review. As a result, four distinct clusters were identified, as visually represented in Figure 7. Cluster 1, shown in red on the map, includes countries such as India, Iran, the Russian Federation, Brazil, Turkey, Italy, Egypt, and Greece. Within this group, India stood out with 14 documents, 15 links, and a total link strength of 382, indicating strong representation and connection in the analyzed network. Iran had seven documents, seven links, and a total strength of 74, suggesting a more modest presence. Brazil contributed with three documents, 11 links, and a strength of 20, indicating more discrete connectivity compared to others in the group. The Russian Federation had two documents, eight links, and a strength of 13. Turkey, with three documents and 13 links, achieved a strength of 101, while Italy, with the same number of documents but nine links, showed a strength of 99. Egypt had five documents, 12 links, and a strength of 188, placing it in an intermediate position in terms of connectivity. Greece presented two documents, 14 links, and a strength of 179, notable for its high number of connections despite modest production. Cluster 2, shown in green, groups Asian countries such as China, South Korea, and Malaysia. China is the most prominent in the group, with 18 documents, 15 links, and a total link strength of 587, revealing strong interconnection and centrality in the network. South Korea, with only four documents, recorded 14 links and a strength of 442, standing out for its high relative connectivity. Malaysia, in turn, had two documents, 12 links, and a strength of 348. Despite a smaller scientific output, both South Korea and Malaysia show relevant network insertion, suggesting thematic affinity and shared references with other countries.
Figure 7. Bibliographic coupling map between countries. Generated using VOSviewer software. 10/14
Polímeros, 36(2), e20260019, 2026
Application of biopolymers in hydrogels for tissue repair with bioextracts: systematic review Cluster 3, in blue, includes Saudi Arabia, United States, and Pakistan. Saudi Arabia stands out with four documents, 14 links, and the highest total link strength of 1056 among all countries, indicating a high density of bibliographic connections. The United States, with six documents, 15 links, and a strength of 802, also shows strong centrality in the network. Pakistan, despite having only two documents, presented 11 links and a strength of 569. This scenario reinforces that link strength is not solely dependent on the number of documents, but on the degree of reference overlap among publications, highlighting thematic proximity and potential indirect collaborations. Cluster 4, shown in yellow, includes France and Tunisia, both with three documents, 12 links, and a total link strength of 323. The similarity in quantitative data and the strength of connections suggest a close scientific relationship, possibly reflecting bilateral collaborations or common use of theoretical and methodological frameworks. The analysis of international collaborations (Figure 7) reinforces this trend, with countries such as China, India, and the United States emerging as leaders in scientific production, driven by specialized journals like the International Journal of Biological Macromolecules. However, the intensity of bibliographic connections among countries varied considerably, reflecting inequalities in international scientific integration[29].
3.7 Keyword co-occurrence analysis Figure 8 presents the keyword analysis, which identified 61 terms distributed across three main thematic clusters,
revealing the structure of scientific production at the interface between biomaterials, pharmacology, and biomedicine. Cluster 1, comprising 26 items and represented in green, includes keywords such as “alginic acid,” “animal experiment,” “in vivo study,” “hydrogel,” “wound healing,” “particle size,” and “porosity.” This group is strongly associated with animal models and preclinical studies, emphasizing the use of hydrophilic materials such as hydrogels for wound therapy. It also encompasses terms related to the physicochemical characterization of materials, such as particle size and porosity. The most relevant journals in this cluster include the International Journal of Biological Macromolecules, with 14 documents and a Total Link Strength of 97, and the Saudi Pharmaceutical Journal, featuring a highlighted article with 104 citations. Cluster 2, made up of 24 items and illustrated in blue, includes terms related to antimicrobial activity (“antibacterial activity,” “staphylococcus aureus,” “escherichia coli”) and the development of controlled drug delivery systems, such as “controlled drug delivery” and “nanofiber.” It also includes keywords related to biocompatibility and the use of synthetic materials, such as “biomaterial” and “nanofibers.” Journals associated with this thematic group include Applied Bio Materials and Materials Advances, both contributing significantly to the topic. Cluster 3, consisting of 11 items and represented in pink, gathers keywords centered on cellular studies and tissue engineering applications, including “cell culture,” “cell viability,” “cytotoxicity,” and “cell proliferation.” This group also covers terms related to the use of biocompatible implants and dressings, such as “gelatin” and “wound dressing”.
Figure 8. Keyword co-occurrence map. Generated using VOSviewer software. Polímeros, 36(2), e20260019, 2026
11/14
Nascimento, O. S., Santana, A. F., Lima, C. S. A., Martins, A. C. S., & Yara, R. The most representative journals in this cluster are Biomaterials Science, with nine citations, and Biomedical Materials, with three published documents. The thematic group related to biomedical materials and functional polymers includes keywords referring to both synthetic and natural materials with medical and pharmaceutical applications, particularly in tissue engineering, wound healing, and controlled drug delivery systems. Noteworthy terms in this context include “hydrogel” (27 occurrences, Total Link Strength: 476), a hydrophilic material widely used in regenerative therapies and drug delivery; “chitosan” (23 occurrences, Total Link Strength: 287), a natural polymer with recognized biocompatible and antimicrobial properties; and “collagen” (12 occurrences, Total Link Strength: 226), a structural component of biological tissues commonly associated with implants and biocompatible matrices. Also worth highlighting is the term “biomaterial” (10 occurrences, Total Link Strength: 184), which broadly designates materials used in tissue engineering. These concepts frequently appear in specialized journals, such as the International Journal of Biological Macromolecules (14 documents) and ACS Applied Bio Materials (1 document), confirming their relevance in studies on smart materials and regenerative therapies. The strong connection between “hydrogel” and “wound healing” (43 co-occurrences, Total Link Strength: 757) underscores the prominence of these materials in promoting cellular regeneration and advancing innovative therapeutic approaches.
3.8 Experimental methodologies used in the studies Of the types of studies conducted in the articles included in the review, it can be seen that the majority of studies carried out in vitro experiments (n = 40), while a significantly smaller number were conducted exclusively in vivo (n = 3). In addition, 32 studies combined in vitro and in vivo approaches, demonstrating the search for greater robustness and validity in the tests carried out with biomaterials. This categorization is essential to understand the complexity and methodological robustness of scientific investigations. In vitro tests are widely used because they allow controlled analyses in laboratory environments, enabling the evaluation of cellular and molecular mechanisms, greater reproducibility, and the absence of ethical concerns related to animal use[30]. On the other hand, in vivo tests are crucial for biological validation in living organisms, offering data on systemic effects, pharmacokinetics, and toxicity that cannot be fully replicated in artificial systems[31]. Studies that combine both methods represent an integrated approach, enhancing the reliability of the results by merging the precision of in vitro tests with the biological complexity of in vivo models[32]. This methodological integration reflects a growing trend in scientific research, which seeks a balance between experimental rigor, clinical applicability, and ethical responsibility. The qualitative analysis identified two predominant conceptual cores: the first focused on the development of biomaterials for wound dressings and healing, with an emphasis on antimicrobial strategies; the second related to tissue engineering, with a focus on bone regeneration and cellular modulation. Both demonstrated a strong 12/14
experimental foundation and biomedical applicability[33], but also highlighted the lack of clinical studies or more robust translational validations[24].
4. Conclusion This systematic review with meta-analysis critically synthesized the scientific evidence on the use of biopolymers incorporated into hydrogels functionalized with bioextracts for tissue repair, providing a comprehensive overview of current trends and gaps in the literature. The analysis revealed a significant growth in scientific output from 2022 onwards, highlighting the strengthening of the field and the consolidation of interdisciplinary approaches involving biomaterials engineering, nanotechnology, pharmaceutics, and regenerative medicine. The data indicate that hydrogels composed of natural biopolymers such as chitosan, alginate, and collagen, when associated with plant- or microbe-derived bioextracts, have relevant therapeutic potential for wound healing, with antimicrobial, antioxidant, and pro-regenerative properties. The predominance of in vitro studies and the increasing use of in vivo models suggest an ongoing effort in scientific translation, although the lack of clinical trials still limits the direct application of these biomaterials in clinical practice. Bibliometric analyses revealed a complex and collaborative scientific network, highlighting strategic institutional centers and high-impact journals, as well as identifying three major thematic axes: wound therapy, controlled drug delivery systems, and tissue engineering. The application of artificial intelligence in the design and optimization of hydrogels emerges as a promising trend to accelerate the development of personalized and efficient biomaterials. Based on these findings, it can be concluded that biofunctionalized hydrogels represent an innovative and versatile therapeutic platform with broad potential for application in regenerative medicine. However, the clinical consolidation of these technologies requires the standardization of experimental protocols, the strengthening of international collaborations, and the conduction of well designed clinical studies. This study contributes to guiding future research, innovation policies, and strategic decision-making in the field of biomaterials applied to healthcare.
5. Author’s Contribution • Conceptualization – Otávio Soares Nascimento; Ana Cristina Silveira Martins. • Data curation – Otávio Soares Nascimento; Ricardo Yara. • Formal analysis – Otávio Soares Nascimento; Ana Cristina Silveira Martins; Adriano Freitas de Santana. • Funding acquisition – NA. • Investigation – Cláudia Sampaio de Andrade Lima. • Methodology – Cláudia Sampaio de Andrade Lima; Ana Cristina Silveira Martins; Ricardo Yara. • Project administration – Ana Cristina Silveira Martins; Ricardo Yara. • Resources – NA. Polímeros, 36(2), e20260019, 2026
Application of biopolymers in hydrogels for tissue repair with bioextracts: systematic review • Software – Otávio Soares Nascimento; Adriano Freitas de Santana. • Supervision – Cláudia Sampaio de Andrade Lima; Ana Cristina Silveira Martins; Ricardo Yara. • Validation – Cláudia Sampaio de Andrade Lima. • Visualization – Cláudia Sampaio de Andrade Lima; Ana Cristina Silveira Martins; Ricardo Yara. • Writing – original draft – NA. • Writing – review and editing – Cláudia Sampaio de Andrade Lima; Ana Cristina Silveira Martins; Ricardo Yara.
7. References 1. Cavalcante, T. S. F., Ferreira, A. K., Amorim, S. J., & Rezende, G. O. (2024). Biotecnologia: avanços na engenharia de tecidos para regeneração de órgãos e tecidos. Revista Contemporânea, 4(10), e5963. https://doi.org/10.56083/RCV4N10-015. 2. Bodla, S., Jain, P., Khanra, A., Sharma, C., Jyoti, A., Purohit, S. D., Singh, H., Singh, A., & Saxena, J. (2025). Biomimetic chitosan-based hydrogels for sustainable wound healing with AI/ML insights. IEEE Open Journal of Engineering in Medicine and Biology, 6, 450-458. https://doi.org/10.1109/ OJEMB.2025.3562382. PMid:40657048. 3. Xu, Z. (2021). Applications of hydrogels in biomedicine. In Proceedings of the 3rd International Academic Exchange Conference on Science and Technology Innovation (IAECST), Guangzhou, China. New York: IEEE. https://doi.org/10.1109/ IAECST54258.2021.9695922. 4. Pankoh, T., Itthipanichpong, R., & Ratanavaraporn, J. (2023). Physical and biological investigation of injectable thai silk fibroin/hyaluronic acid hydrogel sustained-releasing dexamethasone. In Proceedings of the 15th Biomedical Engineering International Conference (BMEiCON), Tokyo, Japan. New York: IEEE. https://doi.org/10.1109/ BMEiCON60347.2023.10322033. 5. Swathy, M., Ramya, E., Shruthi, M. G., Lokeshan, R., & Abinesh, S. (2024). Chitosan based biopatches impregnated with Amaranthus spinosus herbal drug for wound healing application. In Proceedings of the 10th International Conference on Bio Signals, Images, and Instrumentation (ICBSII), Chennai, India. New York: IEEE. https://doi.org/10.1109/ ICBSII61384.2024.10562390. 6. Çelebi, N. N., Bilgiç, E., Sirek, B., Pulat, G., Avşar, N. T., & Karaman, O. (2023). Development of antimicrobial peptide-conjugated GelMa hydrogel-based wound dressing and evaluation of antimicrobial activity. In Proceedings of the 2023 Medical Technologies Congress (TIPTEKNO), Famagusta, Cyprus. New York: IEEE. https://doi.org/10.1109/ TIPTEKNO59875.2023.10359215. 7. Jing, X., Zhang, H., & Liu, D. (2024). Bioactive anti-inflammatory antibacterial plasma-activated hydrogel for infected wound healing. In Proceedings of the IEEE International Conference on Plasma Science (ICOPS), Beijing, China. New York: IEEE. https://doi.org/10.1109/ICOPS58192.2024.10626857. 8. Korzeniewska, E., & Krawczyk, A., SzczęSny, A., Serwach, M., & Mróz, J. (2023). Electroceutical devices in wounded skin treatment. In Proceedings of the 5th International Conference on Modern Electrical and Energy System (MEES), Kremenchuk, Ukraine. New York: IEEE. https://doi.org/10.1109/ MEES61502.2023.10402404. 9. Borschiver, S., Almeida, L. F. M., & Roitman, T. (2008). Monitoramento tecnológico e mercadológico de biopolímeros. Polímeros: Ciência e Tecnologia, 18(3), 256-261. https://doi. org/10.1590/S0104-14282008000300012. Polímeros, 36(2), e20260019, 2026
10. Tariq, Z., Iqbal, D. N., Rizwan, M., Ahmad, M., Faheem, M., & Ahmed, M. (2023). Significance of biopolymer-based hydrogels and their applications in agriculture: a review in perspective of synthesis and their degree of swelling for water holding. RSC Advances, 13(35), 24731-24754. https://doi.org/10.1039/ D3RA03472K. PMid:37601588. 11. Ho, T.-C., Chang, C.-C., Chan, H.-P., Chung, T.-W., Shu, C.-W., Chuang, K.-P., Duh, T.-H., Yang, M.-H., & Tyan, Y.-C. (2022). Hydrogels: properties and applications in biomedicine. Molecules, 27(9), 2902. https://doi.org/10.3390/ molecules27092902. PMid:35566251. 12. Yang, J., Qin, P., & Chen, Z. (2024). Application and prospect of hydrogels in diabetic wound treatment. arXiv, 2406.00297, 1-21. https://doi.org/10.48550/arXiv.2406.00297. 13. Sampaio, R. F., & Mancini, M. C. (2007). Systematic review studies: a guide for careful synthesis of scientific evidence. Revista Brasileira de Fisioterapia, 11(1), 77-82. https://doi. org/10.1590/S1413-35552007000100013. 14. Berwanger, O., Suzumura, E. A., Buehler, A. M., & Oliveira, J. B. (2007). Como avaliar criticamente revisões sistemáticas e metanálises? Revista Brasileira de Terapia Intensiva, 19(4), 475-480. https://doi.org/10.1590/S0103-507X2007000400012. PMid:25310166. 15. Baas, J., Schotten, M., Plume, A., Côté, G., & Karimi, R. (2020). Scopus as a curated, high-quality bibliometric data source for academic research in quantitative science studies. Quantitative Science Studies, 1(1), 377-386. https://doi.org/10.1162/qss_a_00019. 16. Braun, V., & Clarke, V. (2006). Using thematic analysis in psychology. Qualitative Research in Psychology, 3(2), 77-101. https://doi.org/10.1191/1478088706qp063oa. 17. Saiz-Alvarez, J. M. (2024). Innovation management: a bibliometric analysis of 50 years of research using VOSviewer® and Scopus. WORLD, 5(4), 901-928. https://doi.org/10.3390/ world5040046. 18. Donthu, N., Kumar, S., Mukherjee, D., Pandey, N., & Lim, W. M. (2021). How to conduct a bibliometric analysis: an overview and guidelines. Journal of Business Research, 133, 285-296. https://doi.org/10.1016/j.jbusres.2021.04.070. 19. Shehabeldine, A. M., Salem, S. S., Ali, O. M., Abd-Elsalam, K. A., Elkady, F. M., & Hashem, A. H. (2022). Multifunctional silver nanoparticles based on chitosan: antibacterial, antibiofilm, antifungal, antioxidant, and wound-healing activities. Journal of Fungi, 8(6), 612. https://doi.org/10.3390/jof8060612. PMid:35736095. 20. Khoshnevisan, K., Maleki, H., Samadian, H., Doostan, M., & Khorramizadeh, M. R. (2019). Antibacterial and antioxidant assessment of cellulose acetate/polycaprolactone nanofibrous mats impregnated with propolis. International Journal of Biological Macromolecules, 140, 1260-1268. https://doi. org/10.1016/j.ijbiomac.2019.08.207. PMid:31472212. 21. Hu, Z.-C., Lu, J.-Q., Zhang, T.-W., Liang, H.-F., Yuan, H., Su, D.-H., Ding, W., Lian, R.-X., Ge, Y.-X., Liang, B., Dong, J., Zhou, X.-G., & Jiang, L.-B. (2022). Piezoresistive MXene/ Silk fibroin nanocomposite hydrogel for accelerating bone regeneration by re-establishing electrical microenvironment. Bioactive Materials, 22, 1-17. https://doi.org/10.1016/j. bioactmat.2022.08.025. PMid:36203961. 22. Maia, M. F. S., & Caregnato, S. E. (2008). Co-autoria como indicador de redes de colaboração científica. Perspectivas em Ciência da Informação, 13(2), 18-31. https://doi.org/10.1590/ S1413-99362008000200003. 23. Augustine, R., Zahid, A. A., Wang, M., Webster, T. J., & Hasan, A. (2019). Growth factor releasing core-shell polymeric scaffolds for tissue engineering applications. In Proceedings of the 41st Annual International Conference of the IEEE Engineering in Medicine and Biology Society (EMBC), Berlin, Germany. New York: IEEE. https://doi.org/10.1109/EMBC.2019.8857111. 13/14
Nascimento, O. S., Santana, A. F., Lima, C. S. A., Martins, A. C. S., & Yara, R. 24. Binsfeld, P. C. (2024). Ecossistema tecnológico: reflexão sobre pesquisa, inovação, competitividade e regulação. In C. R. M. Leite, L. A. Fernandes, M. F. F. Rosa, M. S. Silva, P. C. Binsfeld, S. J. M. Campos, & S. S. R. F. Rosa (Eds.), Ecossistema de pesquisa, desenvolvimento e inovação tecnológica em saúde (pp. 43-72). Mossoró: Edições UERN. Retrieved in 2025, July 16, from https://portal.uern.br/wp-content/ uploads/sites/14/2024/10/E-book-Ecossistema-de-PesquisaDesenvolvimento-e-Inovacao-Tecnologica-em-Saude.pdf 25. Pereira, R. S., Santos, I. C., Oliveira, K. D. S., & Leão, N. C. A. (2019). Meta-analysis as a research tool: a systematic review of bibliometric studies in administration. RAM. Revista de Administração Mackenzie, 20(5), eRAMG190186. https://doi.org/10.1590/1678-6971/eramg190186. 26. Üstündağ Okur, N., Hökenek, N., Okur, M. E., Ayla, Ş., Yoltaş, A., Siafaka, P. I., & Cevher, E. (2019). An alternative approach to wound healing field; new composite films from natural polymers for mupirocin dermal delivery. Saudi Pharmaceutical Journal, 27(5), 738-752. https://doi.org/10.1016/j.jsps.2019.04.010. PMid:31297030. 27. Sonamuthu, J., Cai, Y., Liu, H., Mohamed Kasim, M. S. M., Vasanthakumar, V. R., Pandi, B., Wang, H., & Yao, J. (2020). MMP-9 responsive dipeptide-tempted natural protein hydrogelbased wound dressings for accelerated healing action of infected diabetic wound. International Journal of Biological Macromolecules, 153, 1058-1069. https://doi.org/10.1016/j. ijbiomac.2019.10.236. PMid:31756486. 28. Kozlowski, D., Andersen, J. P., & Larivière, V. (2023). The decrease in uncited articles and its effect on the concentration of citations. Journal of the Association for Information Science and Technology, 75(2), 188-197. https://doi.org/10.1002/ asi.24852.
14/14
29. Pohl, H. (2024). Using citation-based indicators to compare bilateral research collaborations. Scientometrics, 129(8), 4751-4770. https://doi.org/10.1007/s11192-024-05087-z. 30. Ciapetti, G., Granchi, D., Verri, E., Savarino, L., Cavedagna, D., & Pizzoferrato, A. (1996). Application of a combination of neutral red and amido black staining for rapid, reliable cytotoxicity testing of biomaterials. Biomaterials, 17(13), 1259-1264. https:// doi.org/10.1016/S0142-9612(96)80001-9. PMid:8805972. 31. Rogero, S. O., Lugão, A. B., Ikeda, T. I., & Cruz, Á. S. (2003). Teste in vitro de citotoxicidade: estudo comparativo entre duas metodologias. Materials Research, 6(3), 317-320. https://doi. org/10.1590/S1516-14392003000300003. 32. Bhatia, S. K., & Yetter, A. B. (2008). Correlation of visual in vitro cytotoxicity ratings of biomaterials with quantitative in vitro cell viability measurements. Cell Biology and Toxicology, 24(4), 315-319. https://doi.org/10.1007/s10565-007-9040-z. PMid:17932777. 33. Silva, A. C., & Dominguez, A. G. D. (2024). Avanços e desafios da translação para o Sistema Único de Saúde do dispositivo médico portátil Rapha®. n C. R. M. Leite, L. A. Fernandes, M. F. F. Rosa, M. S. Silva, P. C. Binsfeld, S. J. M. Campos, & S. S. R. F. Rosa (Eds.), Ecossistema de pesquisa, desenvolvimento e inovação tecnológica em saúde (pp. 291-324). Mossoró: Edições UERN. Retrieved in 2025, July 16, from https://portal.uern.br/wp-content/ uploads/sites/14/2024/10/E-book-Ecossistema-de-PesquisaDesenvolvimento-e-Inovacao-Tecnologica-em-Saude.pdf Received: Jul. 16, 2025 Revised: Jan. 19, 2026 Accepted: Feb. 13, 2026 Editor-in-Chief: Sebastião V. Canevarolo
Polímeros, 36(2), e20260019, 2026
ISSN 1678-5169 (Online)
https://doi.org/10.1590/0104-1428.20250081
Thermal and spectroscopic study of irradiated polymeric systems Rochele Klering1 , Thaíses Lima1* , Patricia Araújo2 , Renata Santos1 , Katia Aquino1 and Elmo Araújo1 Laboratório de Polímeros e Nanoestruturas, Departamento de Energia Nuclear, Universidade Federal de Pernambuco – UFPE, Recife, PE, Brasil 2 Departamento de Engenharia Biomédica, Universidade Federal de Pernambuco – UFPE, Recife, PE, Brasil
1
*thaises.lima@ufpe.br
Abstract In this study, different polymer systems, including polycarbonate (PC) and polyethylene-co-vinyl acetate (EVA) formulations, were exposed to gamma radiation. Spectroscopic analysis using FTIR revealed that these polymers retained their functional groups even after high doses of radiation. However, UV-Vis analysis indicated that gamma irradiation caused a significant increase in the yellowing and darkening index of standard PC, attributed to the formation of radiolytic species. The presence of radiostabilizing compounds reduced these effects on optical properties by 45%. Thermogravimetric analysis was conducted to determine parameters for thermal degradation and the activation energy of PC and EVA, showing that gamma irradiation could impact the kinetics of pyrolysis reactions in polymer systems. Keywords: activation energy, EVA, polycarbonate, spectroscopy, thermal analysis. Data Availability: All data supporting the findings of this study are available from the corresponding author upon request. How to cite: Klering, R., Lima, T., Araújo, P., Santos, R., Aquino, K., & Araújo, E. (2026). Thermal and spectroscopic study of irradiated polymeric systems. Polímeros: Ciência e Tecnologia, 36(2), e20260013. https://doi.org/10.1590/0104-1428.20250081
1. Introduction Various polymeric systems are utilized in electronic devices, medical materials exposed to ionizing radiation, and in cables and detectors in high-energy radiation environments. Irradiation can cause structural changes in these polymers, impacting their thermal, optical, and mechanical properties crucial for specific applications. Radioprotective additives are commonly employed in these polymeric systems, but they may also influence thermal or mechanical stability. The investigation of radiolytic effects on the chemical structure of these materials has been the focus of numerous studies, particularly with poly(ethylene-co-vinyl acetate) (EVA), polymethylmethacrylate (PMMA), polyethylene terephthalate (PET), polycarbonate (PC), and other systems[1-4]. Industries such as automotive, packaging, medical instrumentation, and electronics widely use PC due to its versatility. Similarly, the EVA copolymer has multiple uses in food packaging films, composite coatings, and insulating materials for low-voltage electrical cables in nuclear power plants[5-9]. Many applications also involve exposure to highenergy radiation, necessitating attention to the potential effects on the final properties of these materials. When polymers are irradiated, they can undergo crosslinking and chain scission effects, with the predominant effect depending on the molecular structure and irradiation conditions, leading to significant changes in their physical properties[10-15]. Previous
Polímeros, 36(2), e20260013, 2026
studies have shown that in PC, chain scission is the main effect, leading to noticeable yellowing of the material[16-19]. Additionally, various studies have examined the impact of gamma irradiation on compositions containing EVA copolymers[20-23]. De Medeiros reported that for EVA with 25% and 40% vinyl acetate content, doses of up to 10 kGy result in crosslinking as the predominant effect. With doses greater than 30 kGy, no further increase in the influence on the properties of this polymer is observed[4]. The aim of this study is to investigate the impact of gamma irradiation on the physical, optical, and thermal properties of these polymeric systems for use in ionizing radiation environments up to an absorbed dose of 100 kGy. Thermal analysis was conducted to determine the activation energy and thermal parameters of two polycarbonate formulations: polycarbonate without radiolytic additives (PC) and polycarbonate with radiolytic additives (PCADT), as well as ethylene-co-vinyl acetate copolymer with 40% vinyl acetate content (EVA40). Additionally, the study aimed to analyze the effect that radioprotective additives can have on polymer degradation and stability. To gain a deeper understanding of the radiolytic effects on polymer structures, multiple analytical techniques were employed to assess the impact of gamma irradiation on the kinetic models of pyrolysis processes governing polymer
1/9
O O O O O O O O O O O O O O O O
Klering, R., Lima, T., Araújo, P., Santos, R., Aquino, K., & Araújo, E. thermal degradation through the Starink methods and the combination of the Coats-Redfern and Criado methods. Spectroscopic characterization using FTIR and UV-Vis was also carried out on the samples. The results of this study can provide valuable data for the polymer industry, aiding in the understanding of chemical processes and changes in final properties.
Where β is the heating rate ( d T/ d t) and the conversion rate x = ( mi − mf ) / ( m − mf ) , with mi and mf the initial and final weight of each analyzed degradation step, respectively, and m is the weight at temperature T. k(T) is a temperaturedependent function that follows the Arrhenius equation, given by:
2. Materials and Methods
Where Ea is the activation energy, k0 is a pre-exponential factor dependent on the kinetic model of the pyrolysis reaction, and R is the universal gas constant (R = 0.0304 J/mol°C). Combining Equations 1 and 2, the following relationship is obtained:
2.1 Materials Bisphenol A polycarbonate (PC), in the form of 3 mm thick test specimens, was supplied by Unigel S.A. in two formulations: standard PC (with processing additives) and PC-ADT (processing additives and radio-stabilizing additives). Poly(ethylene-co-vinyl acetate), in pellet form, was purchased from Sigma-Aldrich (samples were used as provided), with a composition of 40% vinyl acetate, referred to as EVA40. The samples were gamma-irradiated using a non-attenuated Co-60 source (Gammacell GC220 Excel irradiator - MDS Nordion, Canada) - Eγ ~ 1.25 MeV, dose rate ~ 1.6 kGy/h, dose rate uncertainty = 0.018x10-6 kGy/h (with k = 1, coverage factor) in air at room temperature ~ 27 °C.
2.2 Characterization Fourier transform infrared spectroscopy (FTIR) analysis was performed at a FTIR-4600 Jasco Spectrometer (Japan) equipped with a ZnSe crystal Attenuated Total Reflectance (ATR ProOne) accessory. Experiments were run in 32 scans at 4 cm-1 resolution, in the 4000-500 cm-1 wavenumber range. Spectra UV-Vis were obtained using the V-730 Jasco spectrophotometer (Japan), in the range of 380-800 nm. Additionally, reflectance mode was used to obtain the color parameters (L, a, b) of the samples in order to calculate the yellowing index and total color difference parameters, which indicate the darkening of the material caused by irradiation in the systems under study. The tristimulus values (X, Y, Z) and chromaticity coordinates (x, y) were evaluated according to the CIE - International Commission on Illumination (1931) system. Simultaneous TGA/DSC2 STARe thermoanalyzer (Mettler Toledo - Switzerland) was used for Termogravimetry Analysis (TGA) and the samples were carried out in 70 microliter aluminum oxide crucibles under N2 (~99.5%) atmosphere (20 mLmin-1), a heating rate of 10 °Cmin-1, with a temperature range of 30 - 600 °C. 2.2.1 Determination of activation energy Several methods have been proposed to calculate the activation energy ( Ea ). For polymeric degradation, it is assumed that the conversion rate ( d x/ d t) during a pyrolysis reaction is proportional to the concentration of reacted material. The conversion rate is a product of two functions: conversion fraction f ( x ) and temperature, k (T ) according to Equation 1 [24].
dx dx = β= k (T ) f ( x ) dt dT 2/9
(1)
k ( T ) = k0 e(
β
− Ea / RT )
(2)
dx − E / RT = k0 e( a ) f ( x ) dt
(3)
The integral form of Equation 3 is presented in Equation 4, and from this, many isoconversional methods use mathematical approximations of the temperature integral.
= g ( x)
x
dx
k0
Tf
( − Ea / RT )
e = dT ∫= f ( x) β ∫ 0
0
k0 Ea p ( x ) (4) βR
p ( x ) is an expression for the integral term of the equation. Integral isoconversional methods are based on finding a mathematical approximation of p ( x ) [25]. Some methods are widely used and well-established for determining the activation energy and kinetic models of reactions, including the Coats-Redfern, Criado, FlynnWall-Ozawa (FWO), Friedman (FR), Starink, Akahira and Sunose (KAS) methods, and others[24,26,27]. In this work, a combination of the Coats-Redfern and Criado methods and the Starink method will be used in this work to obtain the activation energy values. Coats-Redfern is a method that uses an asymptotic approach to solve Equation 4, leading to the relationship:
g ( x) kR E ln= ln 0 − a β Ea RT T2
(5)
Criado and co-workers proposed a method that can be used to determine the kinetic model of each process. By combining Equations 3 and 5, an expression is obtained that relates the theoretical characteristic curve of each reaction mechanism (left side of Equation 6) with data obtained through experimental analysis (right side of Equation 6). By comparing the data obtained from each side of this expression, it is possible to determine the kinetic model that describes each experimental process[24].
f ( x) g ( x)
f ( 0.5 ) g ( 0.5 )
= (Tx / T0.5 )
2
( dx / dT ) x ( dx / dT )0.5
(6)
Where 0.5 refers to the data obtained for the conversion rate x = 0.5. Some expressions of f ( x ) and g ( x ) corresponding to each reaction mechanism are presented in Table 1. On the other hand, Starink presented a method that integrates p ( x ) = e −1.0007 x −0.312 / x1.92in Equation 4, leading to a relationship between the heating rate and the inverse of temperature (1/T) presented in the form of Equation 7 [28]. Polímeros, 36(2), e20260013, 2026
Thermal and spectroscopic study of irradiated polymeric systems Table 1. Theorical Kinetic Models[24]. Model
f ( x)
g ( x)
Power Law (P2) Power Law (P3) Avarami-Erofe’ve (A2) Avarami-Erofe’ve (A3) Avarami-Erofe’ve (A4) Contracting Sphere (R2) Contracting Cylinder (R3) One-Dimensional Diffusion (D1) Two-Dimensional Diffusion (D2) Three-Dimensional Diffusion (D3) Ginstling-Brounshtein (D4) First-Order (F1) Second-Order (F2) Third-Order (F3)
2x1/2 3x2/3 2(1-x)[-ln(1-x)]1/2 3(1-x)[-ln(1-x)]2/3 4(1-x)[-ln(1-x)]3/4 2(1-x)1/2 3(1-x)2/3 1/2x [-ln(1-x)]-1 3(1-x)2/3 / [2(1-(1-x)1/3)] 3/2[(1-x)-1/3-1] (1-x) (1-x)2 (1-x)3
x1/2 x1/3 [-ln(1-x)]1/2 [-ln(1-x)]1/3 [-ln(1-x)]1/4 [1-(1-x)1/2] [1-(1-x)1/3] x2 [(1-x)ln(1-x)]+x [1-91-x)1/3]2 1-(2x/3)-(1-x)2/3 -ln(1-x) (1-x)-1-1 [(1-x)-2-1]/2
ln
β T 1.92
E = −1.0008 a +const. RT
(7)
For different conversion rates and using three different heating rates, it is possible to obtain a curve lnβ / T 1.92 versus 1/T. Curve slope, given by −1.0008 Ea / R , can be used to calculate the activation energy of the pyrolysis process in the thermal degradation of the material[28].
3. Results and Discussions 3.1 FTIR analysis FTIR spectra of EVA40 before and after irradiation show the characteristics of some bands associated with the acetate group and the ethylene group (Figure 1). The region at 3302 cm-1 is attributed to the OH group, resulting from the hydrolysis of the acetate group during the processing of the EVA pellets. The region at 2918 cm-1 refers to the C-H bond, and 2850 cm-1 is related to the -CH3 group present in the acetate. Additionally, the presence of the carbonyl group (C=O) is evidenced by the band at 1733cm-1, as well as bands at 1233cm-1 and 1463cm-1, which can indicate the C-O bond present in the acetate and the methylene group (CH2) present in the ethylene[29]. Some studies have shown that high doses of irradiation can lead to the formation of radicals in ethylene-vinyl acetate due to expected crosslinking[4,30]. However, EVA40 did not exhibit changes in functional groups after irradiation, indicating that crosslinking and chain scission processes are not significant in this case. The standard PC and PC-ADT were examined before and after exposure to gamma irradiation. Figure 2A shows the infrared spectrum of polycarbonate without radiolytic additives, revealing characteristic absorption bands of C=O (1771 cm-1) and C-O (1225 cm-1) of the ester group, indicating the polyester nature of the polycarbonate. Additionally, bands at 2972 cm-1 corresponding to the C-H group; 1501 cm-1 corresponding to C=C bonds; and peaks at 1189 and 1004 cm-1 corresponding to the ether (C-O) were observed. Consistent with the literature, the irradiated PC showed a decrease in the intensities of the absorption bands, which Polímeros, 36(2), e20260013, 2026
Figure 1. FTIR spectra of EVA40 before and after gamma irradiation.
could be due to changes in the spatial orientation of the functional groups or the loss of these groups in the chain[16]. Specifically, the reduction in the intensity of the carbonyl group peak (1770 cm-1) may be linked to the chain scission process at the carbonate site, leading to the degradation of the samples[31]. The spectra of PC-ADT indicated that gamma irradiation did not induce significant changes in the main absorption bands of the material (Figure 2B), confirming the efficacy of the radiolytic additives.
3.2 UV-Vis analysis The UV/VIS analysis spectra of EVA40 are shown in Figure 3, with peaks at 407 and 405 cm-1 for EVA before and after irradiation, respectively. These results show that the peak wavelength changes by less than 1% after gamma irradiation. The color intensity or color shifts (ΔYI, ΔE, Δcab ) were calculated and the results show a small variation in the values (Table 2). These findings are in accordance with FTIR results, indicating that there are no significant changes in the polymer structure. 3/9
Klering, R., Lima, T., Araújo, P., Santos, R., Aquino, K., & Araújo, E. Table 2. Optical Parameters of irradiated and non-irradiated polymer systems. Sample EVA40 PC PC-ADT
Dose (kGy) 0 100 0 100 0 100
YI 3.59 2.42 2.88 98.36 15.43 66.60
ΔYI --1.17 -95.48 -51.17
ΔE 3.63 4.08 16.08 38.64 21.33 21.28
ΔCab 1.78 0.99 1.37 37.51 7.05 27.56
Figure 2. FTIR spectra of PC standard (a); and Activated (b), before and after gamma irradiation.
Standard PC exhibits a peak at 393 cm-1, while irradiated PC shows a peak at 402 cm-1 (Figure 4A). This slight shift may be linked to the amount of light reflected or absorbed by the material. PC-ADT displays peaks at 393 cm-1 and 394 cm-1 before and after irradiation, respectively (Figure 4B), indicating no significant change due to the radio-protective additive. Both standard PC and PC-ADT show increased yellowing values (YI and ΔYI) with higher gamma radiation doses (Table 2), suggesting material degradation. Nouh et al. presented a study on PC/PMMA/PVC blends, where the results suggest that chemically active free radicals are likely responsible for the optical color shifts observed. The gamma radiation broke polymer molecules, trapping free radicals with unpaired spins and causing the color changes[32]. The PC with protective additive (PC-ADT) shows a less pronounced increase in yellowing values as expected. However, as anticipated, the PC with protective additive (PC-ADT) exhibits a more subtle change in yellowing values.
3.3 Thermal analysis
Figure 3. Absorbance Spectra for EVA40, before and after gamma irradiation.
EVA40 thermally degrades in two well-defined stages, as shown in Figure 5. The first stage occurs around 320°C and is related to the degradation of vinyl acetate and the formation of acetic acid. The second stage, around 450°C, corresponds to the degradation of the olefinic part of the polymer chains[33,34]. The thermogram of EVA40 shows no significant changes during these two degradation stages after gamma irradiation at a dose of 100 kGy, corroborating with other characterizations of EVA40 that indicate good stability under a high dose of 100 kGy.
Polycarbonate exhibits a single degradation step starting around 500°C, in accordance with the literature[5,35]. The TGA analysis results for both standard and additivated polycarbonate samples indicate no significant changes with the absorption of gamma radiation by the polymer structure. Generally, the onset degradation temperature shows a small change (<3.5%) when comparing before and after irradiation for both standard and additivated PC (Figure 6). In the case of PC-ADT, a less pronounced step
4/9
Polímeros, 36(2), e20260013, 2026
Thermal and spectroscopic study of irradiated polymeric systems
Figure 4. Absorbance Spectra for standard (a); and additivated (b) PC, before and after gamma irradiation.
around 300°C is observed, which may be related to the degradation process of the radioprotective additives. It is worth noting that for both PC systems, the degradation temperature of the polymeric chain begins around 450°C. There are no significant changes in the thermal stability of PC due to the additives or gamma irradiation.
3.4 Determination of activation energy by TGA Criado’s method was utilized to determine the most suitable kinetic model for the pyrolysis process of the EVA40 under study. Once the kinetic model was identified, the activation energy was calculated using the Coats-Redfern method. During this phase, a visual analysis was conducted to select the kinetic model that best fits the material, considering conversion values x ranging from 0.1 to 0.9. The model that exhibited the closest fit between experimental data and the theoretical function was chosen to be incorporated into the Coats-Redfern model. The EVA in its initial degradation stage displayed well-defined models for both non-irradiated and irradiated materials (Figures 7A and 7B). However, it was challenging to determine the model for the second degradation stage (Figures 7C and 7D). It is worth noting that the Coats-Redfern model may introduce errors in the calculation of activation energy, as it relies on kinetic models that can be influenced by phenomena within the polymeric system, such as radiation-induced degradation of the material[36,37]. Table 3 presents the models obtained for the EVA in each stage of degradation before and after irradiation. Additionally, the activation energy (Ea) of the thermal degradation processes was determined using the Starink method. Analyses were conducted at three heating rates (10, 20, and 30 °C/min) to calculate Ea through Equation 7. The slope of the line obtained at each conversion rate (0.1 to 0.9) allowed for the determination of activation energy values at each rate. According to the Starink method, the activation energy of EVA40 was lower for the irradiated material, possibly due to the chain scissions that occurred when the material was exposed to irradiation. Polímeros, 36(2), e20260013, 2026
Figure 5. Thermograms of EVA samples before and after gamma irradiation.
The study on the activation energy with two different methods was also presented for PC, similar to what was done for EVA. Figure 8 presents the models that fit for standard and additivated PC, before and after irradiation. It is noted that PC samples showed well-defined models even after irradiation, and these models were used to determine the Ea using the Coats-Redfern method. Additionally, the activation energy was also determined using the Starink method, and Table 4 shows the Ea values obtained for each method analyzed. It is observed that gamma irradiation in PC markedly influences the Ea of this polymeric system. The radiolytic effects induced by irradiation caused an increase in the Ea of PC. On the other hand, when additivated, the PC shows a reduction in the Ea values, which can be attributed to the main chain scission effects identified in previous studies[38]. The activation energy (Ea) values obtained in this study for PC (using the Starink method) are comparable to the findings of Feng et al.[39] who used the KAS method. It is worth noting that the Ea value determined in this study (289.62 kJ/mol - Criado, D4 model) 5/9
Klering, R., Lima, T., Araújo, P., Santos, R., Aquino, K., & Araújo, E.
Figure 6. Thermograms of (a) standard PC; and (b) additivated PC, before and after gamma irradiation.
Figure 7. Theoretical functions of Kinetic Models by Criado’s Method and experimental data for the first stage of decomposition of (a) non-irradiated; and (b) irradiated EVA40; as well as the second stage of decomposition of (c) non-irradiated; and (d) irradiated EVA40 .
closely aligns with the result reported by Sohel and colleagues[35] (223.89 kJ/mol - Broido, F1 model). It is important to highlight that Sohel et al. did not conduct a thorough investigation to 6/9
determine the optimal kinetic model (as demonstrated in this study) when using the Broido model, which could lead to errors in the Ea calculation due to the incorrect selection of the kinetic Polímeros, 36(2), e20260013, 2026
Thermal and spectroscopic study of irradiated polymeric systems
Figure 8. Theoretical functions of Kinetic Models by Criado’s Method and experimental data for (a) non-irradiated; and (b) irradiated standard PC; (c) non-irradiated; and (d) irradiated PC-ADT. Table 3. Activation Energy values using different methods for EVA samples. Sample
Model
EVA40 0kGy - 1st Step EVA40 0kGy - 2nd Step EVA40 100kGy - 1st Step EVA40 100kGy - 2nd Step
A4 D3 -R2
Activation Energy (kJ/mol) Starink Method Coats-Redfern Method 72.49 56.96 57.14 108.67 148.20 -113.78 128.70
Table 4. Activation Energy values using different methods for PC samples. Sample
Model
PC 0kGy PC 100kGy PC-ADT 0kGy PC-ADT 100kGy
A4 A4 D3 D3
model. Starink[37,40] carried out a comprehensive analysis on the determination of activation energy and compared various methods, concluding that the Starink method offers greater Polímeros, 36(2), e20260013, 2026
Activation Energy (kJ/mol) Starink Method Coats-Redfern Method 61.22 289.62 102.76 296.86 120.21 255.35 88.94 191.99
precision in calculating Ea as it does not rely on the kinetic model and only necessitates three heating rates in thermal analysis for its determination. 7/9
Klering, R., Lima, T., Araújo, P., Santos, R., Aquino, K., & Araújo, E.
4. Conclusions This study utilizes simple techniques to characterize commonly used polymeric systems in research and industries. Spectroscopic analyses aid in understanding the effects of external factors, such as high-dose ionizing radiation and additives, on these systems. The results demonstrate the excellent thermal and structural stability of both polycarbonate and EVA systems under high doses of gamma radiation. Furthermore, a detailed investigation was conducted on the thermal behavior and kinetic parameters of pyrolysis during polymer degradation. The study, utilizing various methods to determine activation energy, demonstrates that the Starink method offers precision and accuracy even in complex systems with multiple degradation steps, as seen in EVA40. It also remains effective when additional factors like additives and radiation exposure are introduced into the polymeric systems. The data presented in this study can enhance our understanding and potential applications of EVA and/or Polycarbonate-based systems in the future.
5. Author’s Contribution ● Conceptualization – Rochele Klering; Patricia Araújo; Elmo Araújo. ● Data curation – Rochele Klering; Thaises Lima; Renata Santos; Patricia Araújo; Elmo Araújo. ● Formal analysis – Rochele Klering; Thaises Lima; Elmo Araújo. ● Funding acquisition – Patricia Araujo; Katia Aquino; Elmo Araújo. ● Investigation – Rochele Klering; Thaises Lima; Patricia Araújo; Elmo Araújo. ● Methodology – Rochele Klering; Thaises Lima; Patricia Araújo; Elmo Araújo. ● Project administration – Patricia Araújo; Elmo Araújo. ● Resources – Rochele Klering; Thaises Lima; Renata Santos; Patricia Araújo; Katia Aquino; Elmo Araújo. ● Software – ● Supervision – Thaises Lima; Patricia Araújo; Elmo Araújo. ● Validation – ● Visualization – ● Writing – original draft – Rochele Klering; Thaises Lima; Renata Santos; Elmo Araújo. ● Writing – review & editing – Rochele Klering; Thaises Lima; Renata Santos; Katia Aquino; Elmo Araújo
6. Acknowledgements The authors are grateful for the financial support from CNPq (Conselho Nacional de Pesquisa e Desenvolvimento Científico e Tecnológico), and FACEPE (Fundação de Amparo à Ciência e Tecnologia de Pernambuco).
7. References 1. Clough, R. L., Gillen, K. T., Malone, G. M., & Wallace, J. S. (1996). Color formation in irradiated polymers. Radiation Physics 8/9
and Chemistry, 48(5), 583-594. https://doi.org/10.1016/0969806X(96)00075-8. 2. Hill, D. J. T., & Whittaker, A. K. (2016). Radiation Chemistry of Polymers. In E.V. Farahani (Eds.), Encyclopedia of polymer science and technology (pp. 1-58). Hoboken: John Wiley & Sons. https://doi.org/10.1002/0471440264.pst488.pub2. 3. Kulkarni, S. S., & Khadke, U. V. (2016). Low energy gamma radiation induced effects on ultrasonic velocity and acoustic parameters in polyvinylidene fluoride solution. Journal of Materials, 2016(1), 8470689. https://doi.org/10.1155/2016/8470689. 4. Medeiros, M. T. S., Lima, T., Araújo, P., & Araújo, E. S. (2025). Gamma-irradiation effects on poly(ethyleneco-vinyl acetate) (EVA). Polímeros, 35(3), e20250028. https://doi. org/10.1590/0104-1428.20240118. 5. Al-Hakami, Y. M. N., Wahab, M. A., Yildirir, E., & Ates, F. (2024). Thermal degradation kinetics, thermodynamics and pyrolysis behaviour of polycarbonate by TGA and Py-GC/ MS. Journal of the Energy Institute, 113, 101499. https://doi. org/10.1016/j.joei.2023.101499. 6. Boguski, J., Przybytniak, G., & Łyczko, K. (2014). New monitoring by thermogravimetry for radiation degradation of EVA. Radiation Physics and Chemistry, 100, 49-53. https:// doi.org/10.1016/j.radphyschem.2014.03.028. 7. Gohil, M., & Joshi, G. (2022). Perspective of polycarbonate composites and blends properties, applications, and future development: A review. In T. Altalhi, & I. Inamuddin (Eds.), Green composites: preparation, properties, and allied applications (pp. 393-424). Amsterdam: Elsevier. https://doi.org/10.1016/ B978-0-323-99643-3.00012-7 8. Kausar, A. (2017). A review of filled and pristine polycarbonate blends and their applications. Journal of Plastic Film & Sheeting, 34(1), 60-97. https://doi.org/10.1177/8756087917691088. 9. Joseph, S., & Focke, W. W. (2011). Poly(ethylene-vinyl covinyl acetate)/clay nanocomposites: Mechanical, morphology, and thermal behavior. Polymer Composites, 32(2), 252-258. https://doi.org/10.1002/pc.21043. 10. Jamalzadeh, M., & Sobkowicz, M. J. (2022). Review of the effects of irradiation treatments on poly(ethylene terephthalate). Polymer Degradation & Stability, 206, 110191. https://doi. org/10.1016/j.polymdegradstab.2022.110191. 11. Burgstaller, C., Höftberger, T., Gallnböck-Wagner, B., & Stadlbauer, W. (2020). Effects of radiation type and dose on the properties of selected polymers. Polymer Engineering and Science, 61(1), 39-54. https://doi.org/10.1002/pen.25553. 12. Naikwadi, A. T., Sharma, B. K., Bhatt, K. D., & Mahanwar, P. A. (2022). Gamma radiation processed polymeric materials for high performance applications: A review. Frontiers in Chemistry, 10, 837111. https://doi.org/10.3389/fchem.2022.837111. PMid:35360545. 13. Sirin, M., Zeybek, M. S., Sirin, K., & Abali, Y. (2022). Effect of gamma irradiation on the thermal and mechanical behaviour of polypropylene and polyethylene blends. Radiation Physics and Chemistry, 194, 110034. https://doi.org/10.1016/j. radphyschem.2022.110034. 14. Elhady, M., Ghobashy, M., & Mahmoud, M. (2020). Effect of gamma irradiation on the adhesive property and antibacterial activity of blend polymer (abietic acid-EVA). Polymers & Polymer Composites, 29(2), 138-147. https://doi. org/10.1177/0967391120904619. 15. Silva, P. P. O., Araujo, P. L. B., Lima, T. B. S., & Araujo, E. S. (2022). The influence of environmental stress cracking (ESC) and gamma irradiation on the mechanical properties of polycarbonate: study of synergistic effects. Materials Research, 25, e20210342. https://doi.org/10.1590/1980-5373-mr-2021-0342. 16. Araújo, E. S., Khoury, H. J., & Silveira, S. V. (1998). Effects of gamma-irradiation on some properties of Durolon polycarbonate. Polímeros, 36(2), e20260013, 2026
Thermal and spectroscopic study of irradiated polymeric systems Radiation Physics and Chemistry, 53(1), 79-84. https://doi. org/10.1016/S0969-806X(97)00300-9. 17. Zaki, M. F., Elmaghraby, E. K., & Elbasaty, A. B. (2015). Structural alterations of polycarbonate/PBT by gamma irradiation for high technology applications. Journal of Adhesion Science and Technology, 30(4), 443-457. https://doi.org/10.1080/016 94243.2015.1105123. 18. Sinha, D., Sahoo, K. L., Sinha, U. B., Swu, T., Chemseddine, A., & Fink, D. (2004). Gamma-induced modifications of polycarbonate polymer. Radiation Effects and Defects in Solids, 159(10), 587595. https://doi.org/10.1080/10420150412331330539. 19. Sharma, T., Aggarwal, S., Sharma, A., Kumar, S., Mittal, V. K., Kalsi, P. C., & Manchanda, V. K. (2008). Modification of optical properties of polycarbonate by gamma irradiation. Radiation Effects and Defects in Solids, 163(2), 161-167. https://doi.org/10.1080/10420150701688503. 20. Girard-Perier, N., Marque, S. R. A., Dupuy, N., Claeys-Bruno, M., Gaston, F., Dorey, S., Fifield, L. S., Ni, Y., Li, D., Fuchs, W. K., Murphy, M. K., Pillai, S. D., Pharr, M., & Nichols, L. (2022). Effects of X-rays, electron beam, and gamma irradiation on chemical and physical properties of EVA multilayer films. Frontiers in Chemistry, 10, 888285. https://doi.org/10.3389/ fchem.2022.888285. PMid:35646817. 21. Gaston, F., Dupuy, N., Marque, S. R. A., Gigmes, D., & Dorey, S. (2018). Monitoring of the discoloration on γ-irradiated PE and EVA films to evaluate antioxidant stability. Journal of Applied Polymer Science, 135(18), 46114. https://doi. org/10.1002/app.46114. 22. Ni, Y., Bisel, T. T., Hasan, M. K., Li, D., Fuchs, W. K., Cooley, S. K., Nichols, L., Pharr, M., Dupuy, N., Marque, S. R. A., Murphy, M. K., Pillai, S. D., Dorey, S., & Fifield, L. S. (2023). Compatibility of ethylene vinyl acetate (EVA)/ethylene vinyl alcohol (EVOH)/EVA films with gamma, electron-beam, and X-ray irradiation. NPJ Materials Degradation, 7(1), 93. https:// doi.org/10.1038/s41529-023-00413-x. 23. Mamdouh, M., El Fadl, F. A., Araby, E., & Ibrahim, S. (2024). Preparation and modification of ethylene vinyl acetate (EVA)/ rosin blends with gamma radiation for antimicrobial applications. Egyptian Journal of Radiation Sciences and Applications, 37(1), 39-54. https://doi.org/10.21608/ejrsa.2024.277944.1167. 24. Aboulkas, A., El Harfi, K., & El Bouadili, A. (2010). Thermal degradation behaviors of polyethylene and polypropylene. Part I: pyrolysis kinetics and mechanisms. Energy Conversion and Management, 51(7), 1363-1369. https://doi.org/10.1016/j. enconman.2009.12.017. 25. Dhyani, V., Kumar, J., & Bhaskar, T. (2017). Thermal decomposition kinetics of sorghum straw via thermogravimetric analysis. Bioresource Technology, 245(Pt A), 1122-1129. https:// doi.org/10.1016/j.biortech.2017.08.189. PMid:28954382. 26. Vyazovkin, S., Burnham, A. K., Criado, J. M., Pérez-Maqueda, L. A., Popescu, C., & Sbirrazzuoli, N. (2011). ICTAC Kinetics Committee recommendations for performing kinetic computations on thermal analysis data. Thermochimica Acta, 520(1-2), 1-19. https://doi.org/10.1016/j.tca.2011.03.034. 27. Criado, J. M., Pérez-Maqueda, L. A., Gotor, F. J., Málek, J., & Koga, N. (2003). A unified theory for the kinetic analysis of solid state reactions under any thermal pathway. Journal of Thermal Analysis and Calorimetry, 72(3), 901-906. https:// doi.org/10.1023/A:1025078501323. 28. Yao, Z., Yu, S., Su, W., Wu, D., Wu, W., & Tang, J. (2020). Kinetic modeling study on the combustion treatment of cathode from spent lithium-ion batteries. Waste Management & Research, 38(1), 100-106. https://doi.org/10.1177/0734242X19879224. PMid:31603400. 29. Madani, M., & El-Sayed, S. M. (2007). Radiation effects on optical properties of ethylene vinyl acetate copolymer films. Polímeros, 36(2), e20260013, 2026
Journal of Macromolecular Science, Part B: Physics, 46(3), 441-451. https://doi.org/10.1080/00222340701257554. 30. Şen, M., & Çopuroğlu, M. (2005). A comparative study of gamma irradiation of poly(ethylene-co-vinyl acetate) and poly(ethylene-co-vinyl acetate)/carbon black mixture. Materials Chemistry and Physics, 93(1), 154-158. https://doi. org/10.1016/j.matchemphys.2005.03.005. 31. Jagtap, S. B., Thorat, A. B., Adsure, K. T., Waghmode, M. S., Mene, R. U., Dhole, S. D., Joshi, R. P., & Kale, G. H. (2025). Antimicrobial properties of pristine and gamma irradiated polycarbonate sheets. Next Materials, 9, 101048. https://doi. org/10.1016/j.nxmate.2025.101048. 32. Nouh, S. A., Ellabban, M. A., Algethami, M., Alsomali, F. A., & Barakat, M. M. E. (2025). Color changes and optical properties of gamma irradiated polycarbonate/poly(methyl methacrylate)/polyvinyl chloride blended polymers: linear and nonlinear optical parameters. Journal of Radiation Research and Applied Sciences, 18(4), 101893. https://doi.org/10.1016/j. jrras.2025.101893. 33. Badiee, A., Ashcroft, I. A., & Wildman, R. D. (2016). The thermo-mechanical degradation of ethylene vinyl acetate used as a solar panel adhesive and encapsulant. International Journal of Adhesion and Adhesives, 68, 212-218. https://doi. org/10.1016/j.ijadhadh.2016.03.008. 34. Stephy, A., Antony, A. M., & Francis, T. (2021). Thermal decomposition kinetics of melt-mixed ethylene-co-vinyl acetate based bio-composites. Materials Today. Chemistry, 21, 100544. https://doi.org/10.1016/j.mtchem.2021.100544. 35. Sohel, M. A., Mondal, A., Arif, P. M., Thomas, S., & Sengupta, A. (2021). Effects of graphene on thermal properties and thermal stability of polycarbonate/graphene nanocomposite. Journal of Thermoplastic Composite Materials, 36(1), 326-344. https://doi.org/10.1177/0892705721997887. 36. Emiola-Sadiq, T., Zhang, L., & Dalai, A. K. (2021). Thermal and kinetic studies on biomass degradation via thermogravimetric analysis: A combination of model-fitting and model-free approach. ACS Omega, 6(34), 22233-22247. https://doi. org/10.1021/acsomega.1c02937. PMid:35252634. 37. Starink, M. J. (2003). The determination of activation energy from linear heating rate experiments: a comparison of the accuracy of isoconversion methods. Thermochimica Acta, 404(1-2), 163-176. https://doi.org/10.1016/S0040-6031(03)00144-8. 38. Silva, P. P. J. C. O., Araújo, P. L. B., Silveira, L. B. B., & Araújo, E. S. (2017). Environmental stress cracking in gammairradiated polycarbonate – a diffusion approach. Radiation Physics and Chemistry, 130, 123-132. https://doi.org/10.1016/j. radphyschem.2016.08.006. 39. Feng, Y., Wang, B., Wang, F., Zhao, Y., Liu, C., Chen, J., & Shen, C. (2014). Thermal degradation mechanism and kinetics of polycarbonate/silica nanocomposites. Polymer Degradation & Stability, 107, 129-138. https://doi.org/10.1016/j. polymdegradstab.2014.05.012. 40. Starink, M. J. (2018). Analysis of hydrogen desorption from linear heating experiments: accuracy of activation energy determinations. International Journal of Hydrogen Energy, 43(13), 6632-6641. https://doi.org/10.1016/j.ijhydene.2018.02.064. Received: Aug. 30, 2025 Revised: Dec. 03, 2025 Accepted: Dec. 16, 2025 Associate Editor: Artur J. M. Valente 9/9
ISSN 1678-5169 (Online)
https://doi.org/10.1590/0104-1428.20250076
From filaments to membranes: additive manufacturing of Ecovio® for oil–water separation Iago Rodrigues de Abreu1 , Fábio Delano Penha Marques Torres2 , Arthur Antônio Sousa Sampaio2 , Rudy Folkersma3 , Laura Hecker de Carvalho4 , Lucas Rafael Carneiro da Silva5 , Tatianny Soares Alves1,2 and Renata Barbosa1,2* Programa de Pós-graduação em Ciência e Engenharia de Materiais, Universidade Federal do Piauí – UFPI, Teresina, PI, Brasil 2 Curso de Engenharia de Materiais, Universidade Federal do Piauí – UFPI, Teresina, PI, Brasil 3 NHL Stenden University of Applied Sciences, Emmen, The Netherlands 4 Programa de Pós-graduação em Ciência e Engenharia de Materiais, Universidade Federal de Campina Grande – UFCG, Campina Grande, PB, Brasil 5 Programa de Pós-graduação em Engenharia de Minas, Metalúrgica e de Materiais, Universidade Federal do Rio Grande do Sul – UFRGS, Porto Alegre, RS, Brasil
1
*rrenatabarbosa@yahoo.com
Abstract This study explored Ecovio®-based filaments and 3D-printed membranes functionalized with zinc oxide (ZnO), biocide (BCD), and carnauba wax (CW) for gravity-driven oil–water separation. Filaments and membranes were produced via fused filament fabrication in grid and triangular geometries and characterized through melt flow index, water absorption, optical microscopy, contact angle, and separation performance. ZnO increased melt flow and long-term water absorption, whereas CW reduced water absorption and increased surface hydrophobicity. Optical microscopy revealed composition-dependent pore architectures ranging from ≈ 355 to 668 µm, directly affecting permeation behavior. Membranes delivered high permeation fluxes, exceeding 1.10 × 107 L·m−2·h−1 under gravity-driven operation. The integrated results showed that tailored filler combinations and infill geometries enable tunable hydrophilicity, porosity, and flux, establishing Ecovio® composites as a sustainable and viable platform for additive manufacturing of oil–water separation membranes. Keywords: 3D printing, biodegradable polymers, filtration membranes. Data Availability: All data supporting the findings of this study are included in this article and its supplementary materials. How to cite: Abreu, I. R., Torres, F. D. P. M., Sampaio, A. A. S., Folkersma, R., Carvalho, L. H., Silva, L. R. C., Alves, T. S., & Barbosa, R. (2026). From filaments to membranes: Additive manufacturing of Ecovio® for oil–water separation. Polímeros: Ciência e Tecnologia, 36(2), e20260014. https://doi.org/10.1590/0104-1428.20250076
1. Introduction The global water shortage crisis stands as one of the most urgent and complex challenges of the 21st century. Water scarcity affects over 40% of the global population, with billions lacking safe water and seasonal shortages impacting billions more[1]. Industrial activities such as petrochemicals, mining, and food processing worsen the crisis by introducing persistent pollutants into water bodies, hindering treatment, and threatening health and ecosystems[2]. Efficient, sustainable, and cost-effective solutions are essential, with membrane filtration standing out for its selective separation, minimal secondary waste, and continuous, automated operation[3]. Advances in membrane technology have broadened industrial and environmental applications. Han et al.[4] employed 3D printing with titanium dioxide (TiO2) and Acrylonitrile Butadiene Styrene (ABS) to develop hydrophilic, oleophobic membranes
Polímeros, 36(2), e20260014, 2026
reusable without performance loss. Irfan et al.[5] modified Polyurethane (PU) sponges by incorporating zinc oxide (ZnO) and Polydimethylsiloxane (PDMS), thereby creating superhydrophobic materials with high absorption capacity for oils and organic solvents, such as diesel and n-hexane. Chen et al.[6] combined electrospinning and spray coating to produce biodegradable Polyvinyl Alcohol (PVA), chitosan, and carnauba wax (CW) membranes effective in oil–water separation and heavy metal removal. Despite advances, membrane filtration still faces challenges affecting efficiency and durability. Balancing permeate flow and solute rejection remains critical, as higher flow often lowers separation efficiency[7]. Fouling from particulates, organics, and microorganisms, caused by adsorption, pore blockage, and cake formation, reduces performance, shortens lifespan, and increases costs[8].
1/9
O O O O O O O O O O O O O O O O
Abreu, I. R., Torres, F. D. P. M., Sampaio, A. A. S., Folkersma, R., Carvalho, L. H., Silva, L. R. C., Alves, T. S., & Barbosa, R. Operational factors such as pH, solute concentration, and concentration polarization, along with intrinsic properties like porosity and surface chemistry, are decisive for performance[9,10]. Additive manufacturing, especially fused filament fabrication (FFF), offers a promising option to conventional membrane production, enabling customized geometries for specific applications and reducing solvent use and environmental impact[4,11]. The limited range of printable materials, especially for high-performance uses, highlights the need for thermoplastic or composite filaments with tailored properties[12]. The Ecovio® blend, combining Poly(Lactic Acid) (PLA) stiffness with Poly(Butylene Adipate-co-Terephthalate) (PBAT) flexibility, exemplifies a versatile option for oil–water separation membranes without compromising structural integrity[13-15]. Functional fillers such as ZnO, biocide (BCD), and CW can expand the applications of biodegradable membranes. ZnO provides broad-spectrum antimicrobial activity with stability and low toxicity[16], while biocides, regulated to meet safety standards, prevent microbial degradation and preserve material quality[17]. CW, from the Copernicia prunifera palm of Northeastern Brazil, contains fatty acid esters and long-chain alcohols that confer hydrophobic and lubricating properties[18]. This study presents oil–water separation membranes produced via 3D printing with Ecovio® filaments functionalized with ZnO, BCD, and CW in grid and triangular geometries. Filaments and membranes were characterized to assess processing and composition effects, confirming the suitability of Ecovio® for additive manufacturing and the feasibility of uniting technical performance with environmental sustainability.
resin (phr), with filler amounts referenced to 100 parts of Ecovio®. Table 1 summarizes the compositions, comprising ZnO at 3 and 5 phr, with a fixed 1 phr content for both BCD and CW[19]. The ZnO contents (3 and 5 phr) were selected based on the group’s prior experience, which demonstrated that these contents maintain stable melt flow and reliable processing, whereas higher amounts hinder extrusion. BCD and CW were fixed at 1 phr, consistent with the group’s established processing window. Thus, all compositions have already been validated for efficient, reproducible processing.
2.2 Membrane production by 3D printing Circular membrane prototypes (41.8 mm diameter, 1.0 mm thickness) were produced employing a Creality 3D® Ender-3 printer (China). Printing parameters, optimized through preliminary tests in UltiMaker Cura® (Figure 1), included two internal geometries: grid[20] and triangular[21], both with 95% fill density, 0.8 mm upper/lower thickness, and 0.2 mm layer height. No solid upper or lower layers were added (0 layers) to preserve permeability. Printing and travel speeds were set to 30 mm/s, with extrusion at 175 °C and table heating at 80 °C. PLA filament with a diameter of ± 1.75 mm was extruded through a 0.4 mm nozzle using “skirt” adhesion mode. These parameters aimed to ensure dimensional accuracy, structural integrity, and functional efficiency. Printed membranes were subsequently characterized.
2.3 Characterization of filaments and membranes The melt flow index (MFI) was determined using the alternative extrusion-based procedure described by Kanabenja et al.[22], in which flow behavior is assessed directly in a 3D-printing system. Although not equivalent to the ISO 1133 plastometer method, this approach provides a reproducible comparative indicator of filament flowability under conditions representative of FFF. Filaments were extruded through a 0.4 mm nozzle of a Creality 3D® printer for 30 s at 180, 190, and 200 °C, and the extrudate was collected and weighed to obtain the mass (m, g). MFI was calculated using Equation 1, where t is the extrusion time (s) and the constant 600 converts the value to g/10 min. This method indicates relative flowability trends despite its inherent limitations.
2. Materials and Methods 2.1 Materials The biodegradable polymer matrix used in this study was Ecovio® F2224 (PBAT/PLA), supplied by BASF (Germany), with a mass density of 1.24–1.26 g/cm3 (ISO 1183), melt volume rate of 3.0–6.5 mL/10 min at 190 °C/5 kg (ISO 1133), and melting temperature ranging from 110 to 155 °C. ZnO powder, biocide Sanitized® MB E 22-70 (BCD), and CW were used as functional fillers and obtained from Dinâmica Química Ltda. (Brazil), Clariant S.A. (Brazil) and Ceras Salustiano (Brazil). Soybean oil (Coamo, Brazil) was used as the model contaminant and dispersed phase in the gravity-driven oil–water separation tests. All fillers were incorporated in parts per hundred
MFI =
600 × m t
(1)
Table 1. Compositions of Ecovio®-based filaments expressed in phr. Compositions EC EC/3ZnO EC/5ZnO EC/3ZnO/1BCD EC/5ZnO/1BCD EC/3ZnO/1BCD/1CW EC/5ZnO/1BCD/1CW
Content (phr) EC 100 100 100 100 100 100 100
ZnO 0 3 5 3 5 3 5
BCD 0 0 0 1 1 1 1
CW 0 0 0 0 0 1 1
Note: EC = Ecovio®.
2/9
Polímeros, 36(2), e20260014, 2026
From filaments to membranes: additive manufacturing of Ecovio® for oil–water separation
Figure 1. Sequential workflow for membrane production by 3D printing.
Figure 2. Apparatus for membrane fixation and gravity-driven oil–water separation.
The water absorption (WA) test was performed according to ASTM D570 using five 30 mm specimens. Samples were oven-dried at 60 °C for 24 h (Solab, Brazil), immersed in deionized water at room temperature, and weighed at 24, 48, 168, 336, 504, 672, 840, 1008, and 1176 h. Before weighing, specimens were gently blotted with low-abrasive absorbent paper. WA was calculated using Equation 2, where mT is the mass (g) after immersion time t (h) and mI is the initial mass (g).
= WA
mt − mi × 100% mi
(2)
The surface morphology of the 3D-printed membrane was examined using a binocular optical microscope (DM500, Leica Microsystems, Germany) operating in reflection mode. The equipment was coupled to an ICC50 E digital camera, enabling image acquisition at 40× magnification with a reference scale of 500 μm. The contact angle (θ) was measured according to ASTM D5725 using a 10 μL distilled water droplet placed on samples conditioned at room temperature. Images were captured after 30 s for liquid–solid interface stabilization, and θ was determined with an ImageJ plug-in (NIH, USA). Polímeros, 36(2), e20260014, 2026
Three samples per composition were analyzed (n = 3), with three readings per sample, and mean values classified the membranes as hydrophilic or hydrophobic. The membranes were evaluated for oil–water separation using a gravity-driven method, as described in previous studies[23-25]. The model effluent was prepared by emulsifying soybean oil and distilled water (1:1 v/v) with a Fisatom mechanical stirrer (713D) at 3000 rpm for 5 min. In each test, 80 mL of emulsion was filtered, and the permeate was collected after 30 s. Separation efficiency, calculated from the ratio between the oil mass after separation (m1, g) and the initial oil mass (m2, g), was determined using Equation 3:
= Separation Efficiency
m1 × 100% m2
(3)
Initially, 40 mL of oil and 40 mL of water were weighed, emulsified, and left to rest for 24 h to allow natural oil separation. The recovered oil was extracted with a pipette, transferred to a pre-weighed beaker, and weighed to determine the final mass. A custom AutoCAD-designed apparatus was used, comprising upper and lower molds, a sealing element, and two perpendicular plastic tubes (90°) for gravity-based operation. A 3D-printed support ensured membrane stability, with the CAD model and assembled device shown in Figure 2. 3/9
Abreu, I. R., Torres, F. D. P. M., Sampaio, A. A. S., Folkersma, R., Carvalho, L. H., Silva, L. R. C., Alves, T. S., & Barbosa, R. The separation flux (J) was calculated using Equation 4, where V is the permeated volume (L), A is the effective filtration area (m2), and Δt is the separation time. All tests used Δt = 30 s (0.0083 h), and J was expressed in L·m−2·h−1 (LMH). J=
V A×∆t
(4)
MFI, WA, and contact angle results were analyzed using OriginLab 2024 software via ANOVA. Tukey’s test (p ≤ 0.05) identified significant differences between sample means.
3. Results and Discussion 3.1 Filament Melt Flow Index (MFI) MFI is a key rheological parameter in additive manufacturing, influencing filament deposition and interlayer adhesion. Excessively high values can impair part filling and integrity. Figure 3 shows MFI results at 180, 190, and 200 °C. The control filament (EC) had the lowest MFI at all temperatures. The incorporation of ZnO increased the MFI of the filaments, indicating a reduction in melt viscosity under shear and suggesting a lubricating effect associated with ZnO–polymer interactions[26]. Although lower melt viscosity favors continuous material flow, deposition quality during FFF also depends on viscoelastic recovery and post-extrusion stability, mechanisms not captured by MFI measurements. In the hybrid compositions EC/3ZnO/1BCD/1CW and EC/5ZnO/1BCD/1CW, the presence of CW reduced MFI relative to the ZnO-only systems, likely because its hydrophobic and nonpolar character limits compatibility with the PBAT/PLA matrix and imposes a physical barrier to chain mobility, modulated by particle morphology and dispersion. Previous studies have shown that ZnO can modify polymer rheology by reducing viscosity and increasing MFI, although the magnitude of this effect is system-dependent. For example, in High-Density Polyethylene (HDPE)-based composites, ZnO may improve the mechanical response without significant changes in MFI[27-29]. In this study, the compositions EC/3ZnO/1BCD, EC/5ZnO/1BCD, EC/3ZnO/1BCD/1CW, and EC/5ZnO/1BCD/1CW exhibited lower MFI (i.e., reduced melt flowability) than the ZnO-only compositions, consistent with the barrier effect imposed by multiple fillers on melt mobility. A similar trend was reported by Yu et al.[30] in PLA composites with lignocellulosic fillers, indicating that, despite distinct chemistries, the fillers here imposed comparable rheological constraints. Adjusting filler features and processing temperature is essential to obtain MFI values suitable for stable FFF and to avoid improper melt flow. The trends observed in Figure 3 confirm these combined influences of composition and temperature on flow behavior.
The EC saturated early, maintaining WA around 2.2% over 1176 h, confirming its low water affinity. Consistently, Osman et al.[31] also reported modest WA in PLA/PBAT systems, with neat PLA reaching only 1.15% and neat PBAT 3.15% after 16 days, while the 75PLA/25PBAT blend stabilized at ≈ 2.94%. In line with these findings, Chaiwutthinan et al.[32] observed that neat PLA, neat PBAT, and 70PLA/30PBAT blend exhibited minimal water uptake (≈ 0.3–0.9%) over 120 days, with significant increases occurring only when hydrophilic fillers were added. Similarly, Chen et al.[33] reported that PLA/PBS/PBAT blends showed intrinsically low water sorption, with WA increasing only when hydrophilic nHA (nanohydroxyapatite) was added. Bellon et al.[34] demonstrated that both PBAT and PLA exhibit very low water sorption capacity, with equilibrium values at water activity (aW) = 0.9 of only 0.081 g/g and 0.089 g/g, respectively. These data support the idea that the behavior of Ecovio®, characterized by early saturation and low water content over time, is typical of PBAT/PLA systems without hydrophilic fillers.
Figure 3. MFI of filaments at different processing temperatures. Bars with the same letter are not significantly different (p > 0.05, Tukey’s test).
3.2 Water Absorption (WA) As shown in Figure 4, WA behavior varied among compositions. In the first 48 h, all compositions showed a slight increase (≈ 0.9–1.8%) associated with initial water uptake driven by surface wettability and capillary transport through superficial microchannels. 4/9
Figure 4. WA of EC-based filaments over 1176 h, showing distinct profiles by composition. Polímeros, 36(2), e20260014, 2026
From filaments to membranes: additive manufacturing of Ecovio® for oil–water separation From 48 to 336 h, WA in ZnO- and BCD-containing compositions increased continuously, after which CW-containing systems stabilized while wax-free systems continued to rise. The filaments EC/3ZnO/1BCD/1CW and EC/5ZnO/1BCD/1CW reached a plateau from ≈ 336 h onward, stabilizing at ≈ 1.7–2.0% due to CW’s hydrophobic barrier effect. Incorporation of ZnO alone (EC/3ZnO and EC/5ZnO) yielded the highest WA (8.0–10.2% at 672–1008 h), likely due to microstructural changes that increase free volume and create diffusion pathways. ZnO’s hydrophilicity and fine particle size enhance capillarity and microchannel formation, intensifying WA[35]. Similar effects occurred in cellulosic composites with hydrophilic fillers, though their magnitude depends on the polymer matrix and aqueous medium, as ionic species can alter diffusion and sorption[36,37]. Compositions with ZnO/BCD but without CW (EC/3ZnO/1BCD and EC/5ZnO/1BCD) showed intermediate WA (5.3–6.3%), stabilizing after 504–672 h due to the balance between hydrophilic ZnO and hydrophobic BCD. Adding CW to these hybrids (EC/3ZnO/1BCD/1CW and EC/5ZnO/1BCD/1CW) further reduced WA, confirming a synergistic barrier effect that limited long-term diffusion. From 336 h onward, statistical analysis showed that ZnO-only composites exhibited markedly higher WA compared to the other compositions. This reflects ZnO’s potential catalytic role in hydrolytic degradation[38], which can benefit short-term biodegradable materials but requires caution for long-term use. Absorption curves showed that filler selection tailors WA. CW improved stability in ZnO- and BCD-based systems in humid environments, while high-ZnO compositions accelerate degradation; balancing hydrophilic–hydrophobic properties optimizes performance and environmental compatibility.
3.3 Optical Microscopy (OM) Optical microscopy enabled direct assessment of pore morphology, revealing that both composition and infill geometry markedly influenced pore size (Table 2). The EC/3ZnO membrane with a grid geometry exhibited the smallest pore diameter (355.4 ± 18.4 µm). The higher MFI of the ZnO-containing filaments (Section 3.1) explains this behavior. The increased MFI indicates lower melt viscosity and greater flowability during FFF, allowing the extruded strands to spread more uniformly and coalesce more effectively at the intersections of the grid pattern. This enhanced flow reduces inter-filament gaps, resulting in smaller, more regular pores than in the neat EC membrane. In contrast, triangular-geometry samples containing BCD (EC/3ZnO/1BCD and EC/5ZnO/1BCD) showed larger pores than the neat EC, suggesting reduced flowability and local instabilities during deposition, which may weaken interlayer bonding and accentuate geometric anisotropy. The incorporation of CW in EC/3ZnO/1BCD/1CW partly reversed this trend in triangular geometry, decreasing the average pore diameter (460.8 ± 8.6 µm) and leading to more uniform and denser pore networks. In grid-type samples, CW produced only moderate changes in average pore size, depending on composition, but systematically improved pore regularity, indicating a smoothing effect on filament contours. Polímeros, 36(2), e20260014, 2026
The OM images in Table 3 corroborated these trends, showing more defined and continuous filament paths in ZnOcontaining grids. In contrast, triangular samples with BCD alone exhibited more irregular pore shapes and discontinuous interfaces. The lower porosity and greater homogeneity in membranes with CW indicated better filament coalescence, likely due to the wax’s lubricating effect. Despite limitations, OM differentiated pore variations and showed that MFI, fillers, and geometry define membrane porosity. These results agree with studies showing that porosity and mesh size strongly influence oil–water separation: Park et al.[39] obtained ≈ 90% efficiency with similar porosity, while Koh et al.[40] highlighted the impact of meshes close to 280 µm on performance and fouling resistance. Thus, the results reinforce the need to adjust composition and printing design to control pore architecture and separation performance of Ecovio®-based membranes.
3.4 Contact Angle (θ) Table 4 shows θ values for membranes in grid and triangular geometries, and Table 5 presents representative droplet profiles. Lower θ indicates greater wettability and water affinity, while higher values denote increased hydrophobicity. The neat EC showed θ values of approximately 62–63° in both geometries, indicating a moderately hydrophilic surface. The incorporation of ZnO alone (EC/3ZnO and EC/5ZnO) produced no significant variation in θ relative to EC (p > 0.05), confirming that ZnO did not meaningfully modify surface wettability under the printing conditions adopted. In contrast, the presence of BCD, especially CW, markedly increased θ, with values ranging from 72 to 81° depending on the geometry. This demonstrated that CW is the dominant hydrophobic component in the compositions, whereas ZnO has minimal influence on surface hydrophilicity. These trends are consistent with the WA results (Section 3.2), which showed that CW-containing filaments exhibited reduced long-term water absorption, confirming the coupling between hydrophobic surface chemistry and diffusion-barrier effects. The increase in θ for the CW-containing systems is attributed to the formation of a hydrophobic surface layer rich in long-chain esters, thereby reducing water-polymer matrix interactions. Additionally, topographical effects associated with particle agglomeration and microvoids may intensify hydrophobicity by promoting partial droplet suspension, as described by the Cassie–Baxter model[41]. Table 2. Average pore diameter of 3D-printed membranes with grid and triangular infills. Compositions
Grid EC 561.8 ± 30.9 EC/3ZnO 355.4 ± 18.4 EC/5ZnO 468.1 ± 38.7 EC/3ZnO/1BCD 523.7 ± 16.4 EC/5ZnO/1BCD 503.3 ± 17.5 EC/3ZnO/1BCD/1CW 503.6 ± 29.3 EC/5ZnO/1BCD/1CW 399.9 ± 43.6
Pore size (µm) Triangular 662.3 ± 53.7 520.2 ± 42.3 588.1 ± 60.9 666.9 ± 25.2 668.6 ± 109.7 460.8 ± 8.6 633.4 ± 23.0
Values are reported as mean ± standard deviation. Note: All pore diameter values are reported in µm, consistent with the microscope scale (500 µm).
5/9
Abreu, I. R., Torres, F. D. P. M., Sampaio, A. A. S., Folkersma, R., Carvalho, L. H., Silva, L. R. C., Alves, T. S., & Barbosa, R. Table 3. Optical micrographs of membranes with different compositions and infill geometries. Compositions EC
Table 5. Representative images of water droplets on the membrane surfaces.
OM (500 µm scale/40× magnification) Grid Triangular
Compositions
Grid
Water droplet Triangular
EC
EC/3ZnO EC/3ZnO
EC/5ZnO
EC/3ZnO/1BCD EC/5ZnO EC/5ZnO/1BCD
EC/3ZnO/1BCD
EC/3ZnO/1BCD/1CW
EC/5ZnO/1BCD/1CW EC/5ZnO/1BCD
EC/3ZnO/1BCD/1CW
EC/5ZnO/1BCD/1CW
The droplet displayed for each membrane is representative of its overall surface wettability.
Representative droplet profiles shown in Table 5 corroborated this behavior, with CW-containing membranes exhibiting more spherical droplets and reduced spreading. Wettability was driven mainly by CW, with minor influence from BCD and negligible effect from ZnO, a distinction essential for interpreting separation performance given the role of hydrophobicity in oil-phase interactions.
3.5 Separation efficiency and separation flux in oil–water systems The micrographs revealed variations in filament contour and continuity, reflecting differences in deposition quality during the printing process.
Table 4. Contact angle of the membranes with different compositions and geometries. Contact angle (°) Grid Triangular EC 62.5c ± 4.1 62.5c ± 0.8 EC/3ZnO 61.5c ± 1.0 63.3c ± 1.0 EC/5ZnO 61.0c ± 5.7 64.9c ± 0.9 EC/3ZnO/1BCD 64.4b,c ± 1.0 64.2c ± 0.5 EC/5ZnO/1BCD 76.2a ± 0.2 78.5a,b ± 1.5 EC/3ZnO/1BCD/1CW 72.2a,b ± 1.8 76.6b ± 2.8 EC/5ZnO/1BCD/1CW 75.2a ± 2.7 81.3a ± 1.7 Values are reported as mean ± standard deviation (n = 3). Groups with the same letter showed no significant difference (p > 0.05, Tukey’s test). Compositions
6/9
Efficient oil–water separation remains a challenge in several sectors, with 3D-printed membranes emerging as a promising solution through customizable structural and surface properties. Figure 5 shows the separation efficiency for soybean oil–water mixtures. Separation efficiency reflects the membrane’s ability to retain oil while allowing water permeation, thus minimizing oil passage. This parameter is crucial to evaluate membrane performance in selective separation processes. Membranes with triangular geometry exhibited comparable efficiencies across compositions, a behavior attributed to their greater internal volume and more uniform pore distribution, which reduces direct contact between the oil–water mixture and the membrane surface. As discussed by Zhang et al.[42], the inherent resolution of the applied method may have reduced the ability to capture subtle structural differences. In general, smaller pores tend to increase separation efficiency by blocking oil droplets while maintaining water permeability[43]. Polímeros, 36(2), e20260014, 2026
From filaments to membranes: additive manufacturing of Ecovio® for oil–water separation The results for EC/3ZnO/1BCD/1CW highlight the potential of 3D printing as a versatile and sustainable route for membrane production. The ability to adjust geometry, optimize compositions, and integrate cost-effective fillers offers a scalable path for industrial and environmental applications. Future studies should optimize printing parameters and interfacial compatibility to enhance reproducibility and performance.
4. Conclusions
Figure 5. Oil–water separation efficiency of 3D-printed membranes.
Table 6. Separation flux of 3D-printed Ecovio® membranes under gravity-driven filtration. J in LMH (L·m−2·h−1) Grid Triangular EC 1.022 × 107 ± 4.103 × 105 9.504 × 106 ± 7.352 × 105 EC/3ZnO 1.048 × 107 ± 3.394 × 105 1.058 × 107 ± 5.878 × 105 EC/5ZnO 1.102 × 107 ± 1.153 × 105 1.130 × 107 ± 2.490 × 105 EC/3ZnO/1BCD 1.141 × 107 ± 4.314 × 105 1.080 × 107 ± 1.882 × 105 EC/5ZnO/1BCD 9.864 × 106 ± 5.764 × 105 9.828 × 106 ± 1.882 × 105 EC/3ZnO/1BCD/1CW 1.199 × 107 ± 3.459 × 105 1.055 × 107 ± 4.103 × 105 EC/5ZnO/1BCD/1CW 1.080 × 107 ± 3.394 × 105 1.076 × 107 ± 1.630 × 105 Compositions
Values are reported as mean ± standard deviation.
On the other hand, grid-type membranes presented more distinct performance variations compared to the EC. Their higher structural regularity enhanced efficiency in selected compositions, particularly those containing ZnO and CW. The influence of composition was evident: membranes with ZnO (EC/3ZnO and EC/5ZnO) exhibited hydrophilic characteristics, as previously confirmed by WA analysis. This hydrophilicity aligns with ZnO’s dual nature, which can be hydrophobic or hydrophilic depending on surface treatment[44]. Incorporation of additional fillers, such as BCD, also influenced performance, reinforcing the need to tailor membrane composition for optimal separation. The EC/3ZnO/1BCD/1CW showed slightly greater oil retention, suggesting that CW acts as an additional barrier to oil passage. Separation flux results (Table 6) exhibited a dependence on pore size (Table 2), similar to efficiency. Across both geometries, flux values for EC/5ZnO were higher than those for EC/3ZnO, consistent with the more uniform pore structures obtained at the higher ZnO content. Variations in flux among the membranes can be associated with differences in hydrophilicity, as supported by contact angle data (Table 4), which influence the formation of water layers on the membrane surface. Additionally, surface topology, particularly porosity, modulated this behavior. Polímeros, 36(2), e20260014, 2026
This study demonstrated that composition and infill geometry decisively governed the processing behavior, morphology, wettability, and separation performance of Ecovio®-based membranes produced by FFF. Filaments with ZnO, BCD, and CW showed distinct MFI behaviors, indicating that the combined effect of these fillers altered melt flow during extrusion and, in turn, influenced filament deposition quality. ZnO increased WA, CW markedly reduced it, and BCD/CW combinations enhanced hydrophobicity, while ZnO alone produced minimal changes in θ. OM confirmed composition–geometry interactions, with pore diameters ranging from ≈ 355 µm in grid structures to 668 µm in triangular patterns, directly influencing gravity-driven separation behavior. The structural differences enabled high permeation fluxes, with representative values of 1.10 × 107 L·m−2·h−1 for selected ZnO-containing compositions. Overall, the results confirmed Ecovio® composites as a sustainable platform for 3D-printed oil–water separation membranes with tunable permeability and selectivity.
5. Author’s Contribution • Conceptualization – Iago Rodrigues de Abreu; Renata Barbosa. • Data curation – Iago Rodrigues de Abreu. • Formal analysis – Iago Rodrigues de Abreu. • Funding acquisition – NA. • Investigation – Iago Rodrigues de Abreu; Fábio Delano Penha Marques Torres; Arthur Antônio Sousa Sampaio. • Methodology – Iago Rodrigues de Abreu; Fábio Delano Penha Marques Torres; Arthur Antônio Sousa Sampaio; Renata Barbosa. • Project administration – Renata Barbosa. • Resources – Renata Barbosa; Tatianny Soares Alves; Rudy Folkersma. • Software – NA. • Supervision – Renata Barbosa; Tatianny Soares Alves. • Validation – Iago Rodrigues de Abreu; Renata Barbosa. • Visualization – Iago Rodrigues de Abreu; Lucas Rafael Carneiro da Silva. • Writing – original draft – Iago Rodrigues de Abreu. • Writing – review & editing – Renata Barbosa; Tatianny Soares Alves; Rudy Folkersma; Laura Hecker de Carvalho; Lucas Rafael Carneiro da Silva. 7/9
Abreu, I. R., Torres, F. D. P. M., Sampaio, A. A. S., Folkersma, R., Carvalho, L. H., Silva, L. R. C., Alves, T. S., & Barbosa, R.
6. Acknowledgements The authors gratefully acknowledge the Federal University of Piauí (UFPI), the Polymers and Conjugated Materials Laboratory (LAPCON), the Piauí State Research Support Foundation (FAPEPI), the National Council for Scientific and Technological Development (CNPq), NHL Stenden University of Applied Sciences, and the Green PAC Polymer Application Centre for their essential support to this study.
7. References 1. Mishra, A., & Tushaus, D. W. (2022). Water scarcity. In N. S. Malik, E. A. Gromova, S. Gupta, & B. Balusamy (Eds.), Legal analytics (pp. 105-116). United Kingdom: Chapman and Hall/CRC. https://doi.org/10.1201/9781003215998-9. 2. Sarkhel, R., & Ganguly, P. (2022). Oil pollution and municipal wastewater treatment: issues and impact. In P. Das, S. Manna, & J. K. Pandey (Eds.), Advances in oil-water separation: a complete guide for physical, chemical, and biochemical processes (pp. 57-64). USA: Elsevier. https://doi.org/10.1016/B978-0-323-89978-9.00016-1. 3. Guo, W., Ngo, H.-H., & Li, J. (2012). A mini-review on membrane fouling. Bioresource Technology, 122, 27-34. https:// doi.org/10.1016/j.biortech.2012.04.089. PMid:22608938. 4. Han, L., Shen, L., Lin, H., Huang, Z., Xu, Y., Li, R., Li, B., Chen, C., Yu, W., & Teng, J. (2023). 3D printing titanium dioxide-acrylonitrile-butadiene-styrene (TiO2-ABS) composite membrane for efficient oil/water separation. Chemosphere, 315, 137791. https://doi.org/10.1016/j.chemosphere.2023.137791. PMid:36623602. 5. Irfan, M., Lakshmi, C. N., & Singh, N. (2023). Superhydrophobic polyurethane sponge modified with polydimethylsiloxane/ zinc oxide-rGO for efficient oil or organic solvent/water separation. Materials Letters, 348, 134668. https://doi.org/10.1016/j. matlet.2023.134668. 6. Chen, S., Li, K., Li, X., Chen, Z., Su, X., Zhang, X., Xie, H., Zhou, Y., & Wu, W. (2024). Degradable polyvinyl alcohol/ chitosan@carnauba wax superhydrophobic composite membrane for water-in-oil emulsion separation and heavy metal adsorption. International Journal of Biological Macromolecules, 280(Pt 2), 135603. https://doi.org/10.1016/j.ijbiomac.2024.135603. PMid:39276879. 7. Belfort, G. (2019). membrane filtration with liquids: a global approach with prior successes, new developments and unresolved challenges. Angewandte Chemie International Edition in English, 58(7), 1892-1902. https://doi.org/10.1002/ anie.201809548. PMid:30370979. 8. Yin-Ru, C., Yu-Jen, L., & Duu-Jong, L. (2019). Membrane fouling during water or wastewater treatments: current research updated. Journal of the Taiwan Institute of Chemical Engineers, 94, 88-96. https://doi.org/10.1016/j.jtice.2017.12.019. 9. Giacobbo, A., Bernardes, A. M., Rosa, M. J. F., & Pinho, M. N. (2018). Concentration polarization in ultrafiltration/ nanofiltration for the recovery of polyphenols from winery wastewaters. Membranes (Basel), 8(3), 46. https://doi. org/10.3390/membranes8030046. PMid:30037095. 10. Abd El-Ghaffar, M. A., & Tieama, H. A. (2017). A review of membranes classifications, configurations, surface modifications, characteristics and its applications in water purification. Chem & Bio Engineering, 2(2), 57-82. http://doi.org/10.11648/j.cbe.20170202.11. 11. Jamal, M. A., Shah, O. R., Ghafoor, U., Qureshi, Y., & Bhutta, M. R. (2024). Additive manufacturing of continuous fiberreinforced polymer composites via fused deposition modelling: a comprehensive review. Polymers, 16(12), 1622. https://doi. org/10.3390/polym16121622. PMid:38931971. 8/9
12. Page, Z. A., & Nelson, A. (2024). Additive manufacturing in polymer science. Journal of Polymer Science, 62(12), 25832584. https://doi.org/10.1002/pol.20240374. 13. Silva, R. N., Santos, M. E. S., Alves, T. S., Silva, L. R. C., Santana, R. M. C., Carvalho, L. H., Oliveira, A. D., & Barbosa, R. (2024). Production and characterization of PLA/PBAT-based films incorporated with natural and maleinized vegetable oils. Polímeros: Ciência e Tecnologia, 34(4), e20240037. https://doi.org/10.1590/0104-1428.20240030. 14. Guo, X., Feng, C., Huang, L., Wang, H., Liu, F., & Li, J. (2025). Superhydrophobic PBAT/PLA fibrous membrane with excellent mechanical performance for highly efficient oil–water separation. Fibers and Polymers, 26(4), 1479-1492. https://doi. org/10.1007/s12221-025-00903-6. 15. Senila, L., Kovacs, E., & Senila, M. (2025). A Review of Polylactic Acid (PLA) and Poly(3-hydroxybutyrate) (PHB) as bio-sourced polymers for membrane production applications. Membranes (Basel), 15(7), 210. https://doi.org/10.3390/ membranes15070210. PMid:40710750. 16. Vagena, I.-A., Gatou, M.-A., Theocharous, G., Pantelis, P., Gazouli, M., Pippa, N., Gorgoulis, V. G., Pavlatou, E. A., & Lagopati, N. (2024). Functionalized ZnO-based nanocomposites for diverse biological applications: current trends and future perspectives. Nanomaterials (Basel, Switzerland), 14(5), 397. https://doi.org/10.3390/ nano14050397. PMid:38470728. 17. Unamuno, V. R., van de Plassche, E., & van der Wal, L. (2024). Biocides. In P. Wexler (Ed.), Encyclopedia of toxicology (pp. 85-89). Cambridge: Academic Press. https://doi.org/10.1016/ B978-0-12-824315-2.00115-9. 18. Freitas, M. M. M. (2011). Obtenção de álcoois de cadeia longa a partir da cera de carnaúba (Master’s thesis). Universidade Federal do Ceará, Fortaleza. Retrieved in 2025, August 29, from https://repositorio.ufc.br/handle/riufc/15888 19. Abreu, I. R., Nascimento, R. S., Jr, Fortes, A. G. D. S., Folkersma, R., Leitão, L. V., Marques, F. D. P., Sampaio, A. A. S., Castro, L. L. R. L., Andrade, D. S. C., Alves, T. S., & Barbosa, R. (2024). Thermal and mechanical properties of filaments for additive manufacturing. Polímeros: Ciência e Tecnologia, 34(3), e20240025. https://doi.org/10.1590/01041428.20240034. 20. Yan, C., Ma, S., Ji, Z., Guo, Y., Liu, Z., Zhang, X., & Wang, X. (2019). 3D printing of an oil/water mixture separator with in situ demulsification and separation. Polymers, 11(5), 774. https://doi.org/10.3390/polym11050774. PMid:31052425. 21. Jonhson, W., Xu, X., Bian, K., Xun, Y., Tan, Y. H., Chen, Z., Zhang, D., & Ding, J. (2022). 3D-printed hierarchical ceramic architectures for ultrafast emulsion treatment and simultaneous oil–water filtration. ACS Materials Letters, 4(4), 740-750. https://doi.org/10.1021/acsmaterialslett.2c00147. 22. Kanabenja, W., Passarapark, K., Subchokpool, T., Nawaaukkaratharnant, N., Román, A. J., Osswald, T. A., Aumnate, C., & Potiyaraj, P. (2022). 3D printing filaments from plasticized Polyhydroxybutyrate/Polylactic acid blends reinforced with hydroxyapatite. Additive Manufacturing, 59 (Pt A), 103130. https://doi.org/10.1016/j.addma.2022.103130. 23. Li, X., Shan, H., Zhang, W., & Li, B. (2020). 3D printed robust superhydrophilic and underwater superoleophobic composite membrane for high efficient oil/water separation. Separation and Purification Technology, 237, 116324. https://doi.org/10.1016/j. seppur.2019.116324. 24. Guo, Y., Luo, B., Wang, X., Liu, S., & Geng, T. (2022). Wettability control and oil/water separation performance of 3D-printed porous materials. Journal of Applied Polymer Science, 139(5), 51570. https://doi.org/10.1002/app.51570. Polímeros, 36(2), e20260014, 2026
From filaments to membranes: additive manufacturing of Ecovio® for oil–water separation 25. Rao, L., You, X., Chen, B., Shen, L., Xu, Y., Zhang, M., Hong, H., Li, R., & Lin, H. (2022). A novel composite membrane for simultaneous separation and catalytic degradation of oil/water emulsion with high performance. Chemosphere, 288(Pt 1), 132490. https://doi. org/10.1016/j.chemosphere.2021.132490. PMid:34624347. 26. Murariu, M., Benali, S., Paint, Y., Dechief, A.-L., Murariu, O., Raquez, J.-M., & Dubois, P. (2021). Adding Value in Production of Multifunctional Polylactide (PLA)–ZnO nanocomposite films through alternative manufacturing methods. Molecules (Basel, Switzerland), 26(7), 2043. https://doi.org/10.3390/ molecules26072043. PMid:33918508. 27. Tan, M. A., Yeoh, C. K., Teh, P. L., Rahim, N. A. A., Song, C. C., & Voon, C. H. (2023). Effect of zinc oxide suspension on the overall filler content of the PLA/ZnO composites and cPLA/ZnO composites. e-Polymers, 23(1), 20228113. https://doi.org/10.1515/epoly-2022-8113. 28. Cherubini, F., Riberti, N., Schiavone, A. M., Davì, F., Furlani, M., Giuliani, A., Barucca, G., Cassani, M. C., Rinaldi, D., & Montalto, L. (2024). Production of composite zinc oxide–polylactic acid radiopaque filaments for fused deposition modeling: first stage of a feasibility study. Materials (Basel), 17(12), 2892. https://doi.org/10.3390/ma17122892. PMid:38930261. 29. Vidakis, N., Petousis, M., Maniadi, A., Papadakis, V., & Moutsopoulou, A. (2022). The impact of zinc oxide micropowder filler on the physical and mechanical response of high-density polyethylene composites in material extrusion 3D printing. Journal of Composites Science, 6(10), 315. https:// doi.org/10.3390/jcs6100315. 30. Yu, W., Li, M., Lei, W., Pu, Y., Sun, K., & Ma, Y. (2022). Effects of Wood Flour (WF) pretreatment and the addition of a toughening agent on the properties of FDM 3D-Printed WF/ Poly(lactic acid) biocomposites. Molecules (Basel, Switzerland), 27(9), 2985. https://doi.org/10.3390/molecules27092985. PMid:35566335. 31. Osman, M. J., Ibrahim, N. A., Sharif, J., & Wan Yunus, W. M. Z. (2014). Study on water absorption and biodegradation of polylactic acid/poly (butylene adipate-co-terephthalate) nanocomposite. ChemXpress, 5(2), 66-72. Retrieved in 2025, August 29, from https://www.tsijournals.com/articles/study-onwater-absorption-and-biodegradation-of-polylactic-acidpolybutylene-adipatecoterephthalate-nanocomposite.pdf 32. Chaiwutthinan, P., Chuayjuljit, S., Srasomsub, S., & Boonmahitthisud, A. (2019). Composites of poly(lactic acid)/ poly(butylene adipate-co-terephthalate) blend with wood fiber and wollastonite: physical properties, morphology, and biodegradability. Journal of Applied Polymer Science, 136(21), 47543. https://doi.org/10.1002/app.47543. 33. Chen, P.-H., Chen, C.-W., Mao, H.-I., Dai, C.-A., Su, C.-S., Tsai, J.-C., & Lin, F.-H. (2023). Bio-based PLA/PBS/PBAT ternary blends with added nanohydroxyapatite: a thermal, physical, and mechanical study. Polymers, 15(23), 4585. https://doi.org/10.3390/polym15234585. PMid:38232012. 34. Bellon, J., Bacoup, F., Marais, S., & Gattin, R. (2025). PLA, PBS, and PBAT Biocomposites—Part A: matrix–filler interactions with agro-industrial waste fillers (Brewer’s Spent Grain, Orange Peel) and their influence on thermal, mechanical, and water
Polímeros, 36(2), e20260014, 2026
sorption properties. Materials (Basel), 18(16), 3867. https:// doi.org/10.3390/ma18163867. PMid:40870185. 35. Ji, P., Wang, C., Jiang, Z., & Wang, H. (2016). Influence of surface modification of zinc oxide nanoparticles on thermal behavior and hydrophilic property of PET–PEG composites. Polymer Composites, 37(6), 1830-1838. https://doi.org/10.1002/ pc.23357. 36. Lavrentyev, I. V., Duboviy, V. K., & Simonova, E. I. (2024). Enhancing water absorption in cellulosic composites through hydrophilization. Izvestiâ Sankt-Peterburgskoj lesotehničeskoj akademii, 249, 285-296. https://doi.org/10.21266/20794304.2024.249.285-296. 37. Memon, M. A., Akhtar, M. W., Shahbaz, R., Gabol, N. M., & Baloch, M. (2022). Preparation of a nano-clay-based super absorbent polymer composite for water absorption applications. Mehran University Research Journal of Engineering and Technology, 41(4), 87-94. https://doi.org/10.22581/muet1982.2204.09. 38. Qu, M., Tu, H., Amarante, M., Song, Y.-Q., & Zhu, S. S. (2014). Zinc oxide nanoparticles catalyze rapid hydrolysis of poly(lactic acid) at low temperatures. Journal of Applied Polymer Science, 131(11), 40287. https://doi.org/10.1002/ app.40287. 39. Park, S., Sung, J., & So, H. (2022). Three-dimensional printingassisted all-in-one surfaces inspired by peristome structures for water–oil separation. Surfaces and Interfaces, 29, 101721. https://doi.org/10.1016/j.surfin.2022.101721. 40. Koh, J. J., Lim, G. J. H., Zhou, X., Zhang, X., Ding, J., & He, C. (2019). 3D-printed antifouling cellulose mesh for highly efficient oil/water separation applications. ACS Applied Materials & Interfaces, 11(14), 13787-13795. https://doi.org/10.1021/ acsami.9b01753. PMid:30884229. 41. Yuan, Y., Choi, S.-O., & Kim, J. (2016). Analysis of contact area between water and irregular fibrous surface for prediction of wettability. RSC Advances, 6(77), 73313-73322. https://doi. org/10.1039/C6RA15389E. 42. Zhang, B., Seong, B., Nguyen, V., & Byun, D. (2016). 3D printing of high-resolution PLAbased structures by hybrid electrohydrodynamic and fused deposition modeling techniques. Journal of Micromechanics and Microengineering, 26(2), 025015. https://doi.org/10.1088/0960-1317/26/2/025015. 43. Melnik, A., Bogoslovtseva, A., Petrova, A., Safonov, A., & Markides, C. N. (2023). Oil–water separation on hydrophobic and superhydrophobic membranes made of stainless steel meshes with fluoropolymer coatings. Water (Basel), 15(7), 1346. https://doi.org/10.3390/w15071346. 44. Kołodziejczak-Radzimska, A., & Jesionowski, T. (2014). Zinc oxide—from synthesis to application: a review. Materials (Basel), 7(4), 2833-2881. https://doi.org/10.3390/ma7042833. PMid:28788596. Received: Aug. 29, 2025 Revised: Dec. 09, 2025 Accepted: Dec. 26, 2025 Editor-in-Chief: Sebastião V. Canevarolo
9/9
ISSN 1678-5169 (Online)
https://doi.org/10.1590/0104-1428.20250102
O Optimization of pultruded hybrid bio-filled glass fiber-reinforced O composites for lightweight forearm application O Rajesh Kumar Chandel , Rahul Vaishya , Anish Kumar Bisht , Anurag Gupta * , O Manoj Kumar Singh and Suchart Siengchin O Punjab Engineering College, Chandigarh, India KIET Deemed to be University, Ghaziabad, Uttar Pradesh, India O Natural Composites Research Group Lab, Department of Materials and Production Engineering, The Sirindhorn International Thai-German Graduate School of Engineering, King Mongkut’s University of O Technology North Bangkok, Bangkok, Thailand O Abstract O In this work the effect of pultrusion process variables i.e. pultrusion die temperature, speed of pulling, and % of a hybrid bio filler (calcium carbonate (CaCO ), bagasse fiber, and carbon black (CB)) on the characteristics of pultruded O glass fiber reinforced polymer (GFRP) composites is discussed. The response parameters, namely ultimate tensile and flexural strength, hardness, and % shrinkage were analyzed to realize the effect of pultrusion process parameters. O A Taguchi L9 orthogonal array was used for single response optimization, and gray relational analysis for multi-response optimization. Results show that pultruded GFRP properties are significantly influenced and improved by optimizing the selected process parameters. An improvement of 31%, 6.5%, and 14.6% is achieved in ultimate tensile strength, O flexural strength, and hardness respectively in comparison to result reported in earlier work by the authors. Results show that process optimization effectively enhances the performance, making them suitable for lightweight forearm O protection applications. O Keywords: hybrid bio filler, pultrusion, optimization, blisters, forearm application. Data Availability: All data supporting the findings of this study are available from the corresponding author upon request. O How to cite: Chandel, R. K., Vaishya, R., Bisht, A. K., Gupta, A., Singh, M. K., & Siengchin, S. (2026). Optimization O of pultruded hybrid bio-filled glass fiber-reinforced composites for lightweight forearm application. Polímeros: Ciência 1
1
1
3
2
3
1
2
3
*anurag.gupta@kiet.edu
3
e Tecnologia, 36(2), e20260015. https://doi.org/10.1590/0104-1428.20250102
1. Introduction Since the 1950s a lot of research work has been carried out by researchers in terms of experimental and analytical research in fiber-reinforced plastic (FRP) composites. Several methods for manufacturing FRP composites have been developed so far and pultrusion is one such method that is a continuous manufacturing process for long profile FRP composites[1]. In the pultrusion process, fiber roving or mats are impregnated with liquid polymer resin before curing in the heated die. Martin et al.[2] discussed how resin gels and hardens around fiber reinforcements during Pultrusion, forming a rigid polymer composite. After exiting the heated die, the composite requires minimal finishing operations like trimming or surface treatment. Further Muthukutti et al.[3] explored the curing behavior of the polymeric matrix (resins) when they are subjected to heat. The study was conducted to achieve better product quality along with improved productivity. Ye et al.[4] discussed an experimental method for finding out the mass and volume fraction properties of pultruded GFRP composite. Madenci et al.[5] developed a theoretical approach for analysis of flexural strength
Polímeros, 36(2), e20260015, 2026
of pultruded GFRP composite beam and validate the theoretical results experimentally. The macro, micro, and kinetic analysis were used to understand the flexural failure of the composite. Lackey and Vaughan[6] reported in their work that frictional force, internal die pressure, and viscous force are the significant pultrusion process parameters influencing the pulling speed. The mechanism of blister formation under the influence of heating die temperature, the speed of pulling, heating die length, and composite thickness was investigated by Ding et al.[7]. Giordano and Nicolais identified the temperature of curing die, the rheological variation of polymeric resin, polymerization reaction, and resin viscosity as the factors which influence the properties of the pultruded composite. Boukhili et al. [8] examined the effect of fillers and low-profile additives (LPA) on mechanical characteristics and profile shrinkage. It was concluded through the study that blister formation is the result of low temperature and a higher pulling speed, but by increasing the curing die length, blister formation can be prevented.
1/11
Chandel, R. K., Vaishya, R., Bisht, A. K., Gupta, A., Singh, M. K., & Siengchin, S. Sathishkumar et al.[9] conducted experimental studies on GFRP composites using recycled glass fiber in combination with virgin glass fiber by varying the reinforcement loading. They investigated the resulting changes in the mechanical properties of the composites and proposed a theoretical model to predict the mechanical behavior of hybrid recycled-virgin GFRP composites. Ramesh et al.[10] compared virgin polylactic acid (PLA) with pomegranate peel particulate-reinforced PLA biocomposites and reported that composites containing 15 wt.% biofiller exhibited a substantial improvement in mechanical properties. SEM analysis further revealed enhanced interfacial bonding between the biofiller and the PLA matrix. Chandran et al.[11] reviewed the effect of varying filler loadings in polymer composites and examined their potential industrial applications, including construction, aerospace, and food processing industries. While various studies have investigated the effects of individual process parameters and filler types, comprehensive research on the combined influence of process optimization and hybrid bio-filler incorporation in pultruded GFRP composites remains limited. Moreover, systematic approaches to identify optimal processing conditions that maximize performance metrics such as tensile strength, flexural strength, and impact resistance are still underexplored. The present study aims to bridge this gap by investigating the synergistic effects of pultrusion parameters and hybrid bio-filler content on the mechanical and physical properties of GFRP composites. Through a structured experimental design and optimization methodology, this work seeks to develop sustainable composite solutions with enhanced performance characteristics, contributing both to material innovation and environmental sustainability.
2. Materials and Method 2.1 Materials The list of raw materials utilized for the manufacturing of pultruded GFRP composites is listed in Table 1 with their specification and properties.
2.2 Selection of process parameters The pultrusion parameters, die temperature, pulling speed, and filler content were selected based on literature and validated through preliminary pilot experiments to define a stable processing window. These parameters are reported to have the strongest influence on resin curing, fiber impregnation, and composite quality. Shokrieh and Aghdami[12] showed that die temperature depends on resin gelation, degradation temperature, and reinforcement effects. Since the polyester resin used degrades at ~300 °C, the upper die temperature was limited below this value. Pilot trials revealed matrix degradation above 250 °C; therefore, the maximum die temperature was fixed at 250 °C. Pulling speeds ranging from 75 to 175 mm/min were initially examined. Pilot experiments indicated that speeds below 100 mm/min caused excessive residence time and matrix degradation at higher temperatures, while speeds above 150 mm/min led to incomplete curing. Hence, a practical range of 100-150 mm/min was selected. According to Bank[13], polyester pultruded FRP typically contains 10-30% filler. Based on pilot trials ensuring proper fiber impregnation and avoiding excessive viscosity, three filler levels, 10%, 15%, and 20% were chosen. The finalized parameter levels derived from literature and pilot experimentation are summarized in Table 2.
Table 1. Material used for manufacturing composites and their properties. Material
Property (Value) Viscosity (25 °C): 500 cP, Specific gravity: 1.3, Reticulation operational time (25 °C): 25 min, Young’s modulus: 3.25 GPa, Tensile strength: 50 MPa, Glass transition temperature: 150 °C Reinforcement E glass fiber roving Saint Gobain Ltd. India Specific gravity: 2.35, Diameter: 20-75 µm, Tensile strength: 700-1000 MPa, Elastic modulus: 55 GPa Catalyst for polyester resin Methyl ethyl ketone peroxide Revex Plasticizers (Pvt.) Ltd. India % of active oxygen: 8-9 Accelerator for polyester resin Cobalt Naphtholate Revex Plasticizers (Pvt.) Ltd. India Concentration (6%) Fillers Hybrid filler Bagasse fiber: carbon black: CaCO3: 2.33:1:5 Bagasse fiber Mansurpur Sugar Mills Limited, Average fiber diameter 13 µm and length 60 µm Muzaffarnagar U.P, India CaCO3 Unichem Polymers Pvt. Ltd., U.P., India Particle size: 100 µm Carbon black Jai Enterprises, New Delhi, India Particle size: 50 µm Matrix
Type Source of material Unsaturated polyester resin Revex Plasticizers (Pvt.) Ltd. India
Table 2. Levels of pultrusion parameters used for pultruded GFRP composite fabrication. Variable parameters
Constant parameters
2/11
Levels 1 2 3 Die Temperature (°C) 150 200 250 Pulling speed (mm/min) 100 125 150 Content of hybrid bio filler (%) 10 15 20 Composition of hybrid filler (Bagasse fiber: Carbon black: CaCO3: 2.33: 1: 5), Fiber to resin ratio: 0.95 to 0.96, Catalyst: 1.5% of resin weight, Accelerator: 1% of resin weight
Polímeros, 36(2), e20260015, 2026
Optimization of pultruded hybrid bio-filled glass fiber-reinforced composites for lightweight forearm application 2.3 Manufacturing of pultruded GFRP composite bar Once the process parameters were identified and their level was fixed, a total of 9 experiments according to Taguchi L9 orthogonal array were performed. Three repetitions of each experiment were carried out. A total of 27 rectangular bars of 25 × 10 × 1000 mm3 GFRP bars were pultruded on indigenous pultrusion setup as shown in Figure 1. As Gupta et al.[1] investigated the individual effects of bagasse fiber, carbon black, and CaCO3 on composite performance and optimized their composition to achieve improved mechanical properties at constant die temperature and pulling speed. The optimal hybrid filler composition identified in their study has been adopted in the present work, as mentioned in Table 2. Three blends of unsaturated polyester resin with 10%, 15%, and 20% hybrid bio filler were prepared. The speed and die temperature were controlled as per the design of the experiment and 1% accelerator and 1.5% catalyst were also added to the resin blend. The glass fiber from the creel was dipped in the resin bath and pulled against the heated die by pulling mechanism and the roller pressure during all the experiments were kept uniform. Once the resin-impregnated glass fiber roving passes through the hot die, a cured GFRP composite bar is achieved which was pulled through a pulling mechanism containing rollers.
2.4 Testing of pultruded GFRP composite 2.4.1 Ultimate tensile strength The specimen of pultruded GFRP bars were made as per ASTM D638[14] and tested on a universal testing machine (UTM) of 40 × 103 kg capacity. The strain rate was kept 2 mm/min while conducting the tensile test on a pultruded GFRP composite specimen. The fractured specimens after tensile testing are shown in Figure 1a. 2.4.2 Flexural strength To test the flexural strength of pultruded GFRP composite bars, the three-point flexural test was carried out as per ASTM D790 Standard on UTM[15]. The span and crosshead speed during the test were kept 100 mm and 2 mm/min respectively. The fractured pultruded GFRP composite specimens are shown in Figure 1c
Flexural strength (FS) was calculated using Equation 1:
FS =
3FL
(1)
2bt 2
where F is the load applied on the specimen; L is the span length in mm; b is width of the specimen (mm) and t is the specimen thickness in mm. 2.4.3 Hardness testing To determine the hardness of the pultruded GFRP bar, Rockwell hardness test was carried out as per ASTM D785[16]. A steel ball indenter of diameter 1/8 inch was used, and reading was taken on the Rockwell K scale. 2.4.4 Shrinkage test The shrinkage in the pultruded GFRP composite bar was measured as the variation in the cross-section of the pultrusion die and the cross-section of the pultruded GFRP bar. The % shrinkage of pultruded GFRP composite was determined using Equation 2.
Percentage shrinkage =
( adie − abar ) × 100 adie
(2)
where adie is the die cross-sectional area, which is multiplication product of width of the rectangular die hole (bdie) and thickness of rectangular die hole (tdie). The cross-sectional area of pultruded GFRP composite (abar) is multiplication product of actual width of GFRP bar (bbar) and actual thickness of GFRP bar. 2.4.5 Fiber to resin ratio confirmation test The burnout test was performed to confirm the fiber to resin ratio. The small test specimens were cut from the pultruded GFRP bars of 50 g. The specimen was then put into the muffle furnace at 600 °C for 1 h so that the polyester resin burns out and evaporates. The residue of the specimen after burning was taken out which carries glass fiber and hybrid bio fillers were weighed on a weighing machine having an accuracy of 0.1 mg. To know the fiber weight, the three fillers i.e. CaCO3, bagasse, and carbon black were separately burned out at 600 °C. Weight loss of 80% was found in the bagasse fiber but no significant weight loss was reported in carbon black and CaCO3 fillers.
Figure 1. (a) Indigenous pultrusion setup (b)Tensile fractured pultruded GFRP composites (c) Bending fracture of pultruded GFRP composites Polímeros, 36(2), e20260015, 2026
3/11
Chandel, R. K., Vaishya, R., Bisht, A. K., Gupta, A., Singh, M. K., & Siengchin, S. By weighing the residue pultruded GFRP specimen and subtracting the residue filler weight it was confirmed that the fiber to resin ratio is in the range of 0.96: 1 to 0.99: 1.
2.5 Grey relational grade analysis (GRGA) for multi response optimization GRGA methodology is applied for multi response analysis (MRO), which is helpful to convert an MRO problem into an SRO problem. The experimental data first normalizing in the range from “0” to “1”. The “larger the better” type response are normalized by Equation 3 and “smaller the better” type responses are normalized by Equation 4[17].
x* ( k ) = x* ( k ) =
xi ( j ) − min xi ( j )
(6)
i =1
The optimum parameter setting for MRO was identified corresponding to the highest value of Γ i out of all the GRG. The validity of experimentation was checked by calculating the predicted GRG by Equation 7.
Γ i = Γm +
q
∑ (Γ − Γ ) i
1
(7)
m
where Γm= overall mean of the GRG; Γ i = GRG at the optimal level, q = number of significant process parameters
3. Result and Discussion
max xi ( j ) − xi ( j )
(4)
max xi ( j ) − min xi ( j )
∆ min + ϖ∆max ∆ 0i + ϖ∆max
()
q
∑ ξi ( j)
(3)
max yi ( j ) − min xi ( kj )
where i = 1,2,3, . .n; j = 1,2,3,4. . .Q; n = number of experimental data; Q = number of responses; xi(j) = original sequence; xi*(j)= value after gray relational generation; min xi(k), max xi(k) are the minimum and maximum value of xi(j), respectively. The gray relational coefficient ξi(j) was calculated using Equation 5 for getting the relationship between ideal and actual normalized experimental results.
ξi ( j)=
Γi = 1/ n
(5)
( )
∆ 0i xo* j − x *i j ; xo*(j) = ideal (reference) where = sequence, Δmax = maximum value of Δoi (j), Δmin = minimum value of Δoi (j), ϖ = 0.5, as equal weightage is given to all response characteristics. The gray relation grades (GRG) for each response were calculated by putting the average of gray relational coefficient ξi(j) of each response in Equation 6.
The pultruded GFRP composite specimens were processed as per the experimental scheme given in Table 3. Testing was conducted on the produced specimens to study the effect of process parameters over the various selected output response characteristics. Each trial was repeated three times resulting in 27 specimens. The experimental results for UTS, flexural strength, hardness, and shrinkage along with the S/N ratio are given in Table 3. For the single response optimization, the Taguchi optimization technique was used and the average value of raw data and signal to noise (S/N) ratio of selectedresponse characteristics UTS, flexural strength, hardness, and % shrinkage was calculated from experimental data and presented in Tables 4 to 7, respectively. The S/N ratio and raw data of UTS, flexural strength, hardness, and % shrinkage, respectively is plotted against the process parameter levels. Figure 2 shows the response curves for UTS and it can be found from the curve that the UTS of pultruded GFRP composite increases as the die temperature rises from level 1 to level 3. The higher temperature provides better bonding in between reinforcement, hybrid bio filler, and resin by eliminating moisture content from the hygroscopic carbon black and bagasse fiber present in the hybrid bio filler.
4/11
150 150 150 200 200 200 250 250 250
100 125 150 100 125 150 100 125 150 Mean
10 15 20 15 20 10 20 10 15
(MPa) 309.84 286.88 208.79 335.86 278.04 305.45 276.52 355.64 307.25 296.03
(MPa) 256.91 277.01 248.49 328.83 315.50 261.92 343.35 291.43 315.18 293.18
2.10 1.76 1.46 2.65 1.56 2.99 3.61 2.30 3.11
(db) (HRK) (db) 48.2 54.3 0.58 34.69 48.68 79.3 0.58 37.95 47.91 40.7 0.58 32.1 50.34 94.0 1.00 39.46 49.98 78.3 0.58 37.87 48.36 58.7 0.58 35.34 50.71 61.3 0.58 35.74 49.29 73.0 1.00 37.24 49.97 77.3 0.58 37.79 68.42
5.62 3.58 4.28 3.27 2.64 4.75 3.74 4.61 3.84 4.04
0.13 0.09 0.06 0.08 0.07 0.08 0.09 0.06 0.11
S/N ratio
St. dv.
Average% shrinkage
S/N ratio
St. dv.
Average hardness
(db) 49.72 49.45 46.39 50.26 48.93 49.7 48.5 51.02 49.75
S/N ratio
1.62 2.50 0.70 2.65 1.28 3.36 1.71 2.25 2.64
St. dv.
% of hybrid bio filler
Average flexural strength
Pulling speed (mm/min)
S/N ratio
1 2 3 4 5 6 7 8 9
Die temperature (°C)
St. dv.
Run
Trial conditions
Average tensile strength
Table 3. Taguchi L9 orthogonal array design with selected responses (raw data) and S/N ratio for pultruded GFRP composites.
(db) −14.99 −11.05 −12.72 −10.17 −8.44 −13.54 −11.55 −13.28 −11.68 11.93
Polímeros, 36(2), e20260015, 2026
Optimization of pultruded hybrid bio-filled glass fiber-reinforced composites for lightweight forearm application Table 4. Average values and main effects of ultimate tensile strength (UTS). Level 1 2 3 Delta Rank
Die temperature 48.46 49.70 49.87 1.41 2
Average S/N ratio of UTS Average UTS (raw data) Pulling speed Hybrid bio filler % Die temperature Pulling speed Hybrid bio filler % 49.73 50.18 268.51 307.41 323.64 49.69 49.81 306.45 306.86 309.99 48.61 48.04 313.14 273.83 254.45 1.11 2.14 37.94 33.03 55.54 3 1 2 3 1
Table 5. Average values and main effects of flexural strength. Levels 1 2 3 Delta Rank
Die temperature 48.32 49.56 49.99 1.67 1
Average S/N ratio Pulling speed Hybrid bio filler % 49.75 48.62 49.37 49.72 48.75 49.53 1.00 1.10 3 2
Average flexural strength (raw data) Die temperature Pulling speed Hybrid bio filler % 260.80 309.70 270.09 302.08 294.65 307.01 316.66 275.20 302.45 55.85 34.50 36.92 1 3 2
Table 6. Average values and main effects of hardness. Levels 1 2 3 Delta Rank
Die temperature 34.91 37.56 36.92 2.65 2
Average S/N ratio Pulling speed 36.63 37.69 35.07 2.62 3
Hybrid bio filler % 35.75 38.40 35.23 3.17 1
Average hardness (raw data) Die temperature Pulling speed Hybrid bio filler % 57.83 69.83 61.83 76.92 76.67 83.50 70.50 58.75 59.92 19.09 17.92 23.58 2 3 1
Table 7. Average values and main effects of percentage shrinkage. Level 1 2 3 Delta Rank
Die temperature −12.90 −10.76 −12.14 2.14 2
S/N ratio Pulling speed −12.24 −10.94 −12.61 1.68 3
Hybrid bio filler % −13.94 −11.02 −10.84 3.10 1
Average % shrinkage (raw data) Die temperature Pulling speed Hybrid bio filler % 4.49 4.21 4.99 3.55 3.61 3.56 4.06 4.29 3.55 0.94 0.68 1.43 2 3 1
Figure 2. S/N Ratio and raw data plot for UTS of pultruded GFRP composites. Polímeros, 36(2), e20260015, 2026
5/11
Chandel, R. K., Vaishya, R., Bisht, A. K., Gupta, A., Singh, M. K., & Siengchin, S. It was also observed that the increase in UTS was higher for the die temperature level 1 to level 2 as compared to level 2 to level 3. The mean UTS and S/N ratio of pultruded GFRP was reduced when pulling speed increased from level 1 to level 3 as shown in Figure 2. Almost negligible reduction was observed in the UTS when the pulling speed increased from level 1 to level 2. The slight reduction in UTS was attributed to the possibility of the presence of small uncured patches in pultruded GFRP composite due to an increase in pulling speed. Further, it was found that the UTS reduced considerably as the pulling speed increased from level 2 to level 3. The SEM image of tensile fractured samples of experiment run 8, 2 and 3 shown in Figure 3. The difference between the degrees of bonding can be seen by tensile fractured samples shown in Figure 2 and the SEM images of specimens of the experiment run 8 and 2 in Figures 3a and 3b, respectively. The specimen of the experiment run 8 pulled at pultrusion die temperature Figureows no fiber pull out due to better bonding between glass fiber, polyester resin, and hybrid bio filler. While the specimen of the experiment run 2 pulled at 150 °C shows fiber pullout during tensile loading due to lack of bonding between fiber bio filler and polyester resin. Moreover, the reduction of UTS was due to the blister formation. The higher blister formation was observed at higher pulling speed because the polyester resin could not be cured at the core of the profile. But the upper surface gets cured due to direct contact with heating die and resulted in blister formation[6]. The image of the specimen of the experiment run 7, 8 and 9 is shown in Figure 3d, which has blister formation due to uncured resin coming at the
side surface of the composite because of the pultrusion die pressure. The fibers become compacted due to the increased viscosity of the polyester resin in the pultrusion process causing the reduction in the transverse permeability of the fibers and thus affect the wetting behavior which confirms the finding of Shakya et al.[18]. Samples exhibiting higher strength and stiffness show a dense, uniform microstructure with good fiber-matrix adhesion and minimal voids, whereas specimens with reduced mechanical performance reveal voids, filler agglomeration, and localized blistering. These defects act as stress concentrators, explaining the observed decline in tensile and flexural properties under non-optimal processing conditions. It is also found that with the increase of hybrid bio filler in the composite, higher fibrillation was observed by particulate filler. Higher fibrillation leads to the larger quantity of fiber ends available for crack initiation. Figure 4 shows that as the die temperature increased from level 1 to level 3, the flexural strength of pultruded GFRP increases due to better bonding between filler, reinforcement, and polyester resin matrix. The increase in flexural strength was observed more when die temperature increases from level 1 to 2 as compared to that from level 2 to level 3. This reduction is due to the development of a few micro voids in composite at higher temperatures. The flexural strength of pultruded GFRP composite reduced as the pulling speed was increased. A considerable reduction in flexural strength was observed even when the pulling speed increased from level 1 to 2. The flexural strength of the pultruded GFRP increased with the increase of hybrid bio filler from level 1 to level 2.
Figure 3. SEM fractograph of tensile fractured specimen of (a) experiment run 8; (b) experiment run 2; (c) experiment run 3; (d) Blister formation at the edge of specimens 7, 8 and 9.
Figure 4. S/N ratio and raw data plot for flexural strength of pultruded GFRP composites. 6/11
Polímeros, 36(2), e20260015, 2026
Optimization of pultruded hybrid bio-filled glass fiber-reinforced composites for lightweight forearm application This may be due to the particulate constituents of hybrid bio filler act as stress transfer element in the direction of flexural load. This provides better stress transfer between the glass fiber filaments even though there is a slight compromise with fiber wetting as shown in Figure 5a. It is evident from SEM micrograph of flexural fractured sample of experiment run 3 shown in Figure 5b that as the hybrid bio filler increased further from level 2 to level 3, agglomerations of CaCO3 and carbon black particle present in the hybrid bio filler start damaging the glass fiber filaments coupled with crack initiation. The main effects plot in Figure 6 shows that the hardness of pultruded GFRP composite increases from level 1 of die temperature to level 2 because of the better curing of composite from the surface to core. As the die temperature increases from level 2 to level 3, the curing of the matrix was faster than the core which causes micro void formation inside the profile of the pultruded GFRP leading to a slight reduction of hardness. The percentage of hybrid bio fillers increases the hardness first due to better compaction of fibers as it increases the reinforcement and reduces the void formation. As the hybrid bio filler further increases from level 2 to level 3, the viscosity of the matrix increases causing poor wet out of the fiber, and agglomeration of CaCO3 particles present in hybrid bio filler reduces the hardness of pultruded GFRP composites.
The plot in Figure 7 shows that the shrinkage of the pultruded GFRP composite reduced as the temperature increased from level 1 to level 2. This is because the pultruded GFRP composite cannot cure completely till the core at a low temperature. The shrinkage increases from level 2 to level 3 of temperature because the upper thin layer of the matrix got damaged due to overheating. The main effects plot for % shrinkage in Figure 8 shows that the shrinkage was higher at level 1, and level 3 as compared to shrinkage at level 2 of pulling speed. The damage of the upper layer of the matrix is because of long-time exposure to heat at a low pulling speed of 100 mm/min and post-curing outside the die at a pulling speed of 150 mm/min causes higher shrinkage. It was found that there was a balance between overheating of composite and degree of cure which resulted in a reduction in shrinkage there at a medium pulling speed of 125 mm/min. Figure 7 shows that the increase of hybrid bio filler % reduces the shrinkage as it provides better compaction in pultruded GFRP composite during pultrusion and reduces the void formation inside the composite. The higher hybrid bio filler content increases the resin viscosity which causes the poor wetting of the fiber. Because of poor wetting of the fiber, the less reduction in % shrinkage was observed as % of hybrid bio filler increases from level 2 to level 3.
Figure 5. SEM micrographs of flexural fractured samples of experiment (a) run 2; (b) run 3.
Figure 6. S/N ratio and raw data plot for hardness of pultruded GFRP composites. Polímeros, 36(2), e20260015, 2026
7/11
Chandel, R. K., Vaishya, R., Bisht, A. K., Gupta, A., Singh, M. K., & Siengchin, S.
Figure 7. S/N ratio and raw data plot for percentage shrinkage of pultruded GFRP composites.
Figure 8. Response plot for Grey Relational Grade of pultruded GFRP composites.
Table 8. ANOVA for S/N ratio of UTS and flexural strength. Degree of Freedom (DOF) Sum of square Die temp. temperature 2 3.5667 Pulling speed 2 2.3880 Hybrid bio filler % 2 7.8698 Error 2 0.1024 T 8 13.9268 Process parameter
UTS V F-Ratio 1.7833 34.83* 1.1940 23.32* 3.9349 76.85* 0.0512 -
P (%) 25.61 17.15 56.51 0.74 100
Flexural strength Sum of square V F-Ratio 4.5370 2.2685 71.34* 1.5409 0.7705 24.23* 2.0947 1.0473 32.93* 0.0637 0.0318
P (%) 55.09 18.71 25.43 0.77
*Factors are significant at 95% confidence level; V = Variance; P (%) = % contribution; F-Ratio= statistical test value calculated in ANOVA to determine if group means differ significantly.
The analysis of variance (ANOVA) of S/N ratio data and raw data was carried out to recognize the significant process variables and to quantify their effects on the particular response characteristics. The optimal settings of process variables in terms of mean response data were established by ANOVA and analyzing the main effects plot (Table 8). It is found from ANOVA analysis shown in Table 8 to 11 that the F ratio calculated is greater than the F-ratio table so all three selected pultrusion parameters significant for all four response parameter in both S/N ratio and raw data. ANOVA results directly inform practical process control in pultrusion by identifying the most sensitive parameters. Hybrid bio-filler content shows the highest contribution to UTS, hardness, and shrinkage (44-65%), indicating that filler loading must be tightly controlled to ensure mechanical performance and dimensional stability. Die temperature dominates flexural strength (54-55%), highlighting its critical role in achieving uniform curing and interfacial bonding. Pulling speed exhibits a comparatively lower 8/11
but significant contribution (13-26%) and can therefore be adjusted within a limited range to balance productivity without major performance loss. The SRO determines the optimum process parameter setting for corresponding to the respective output responses and is summarized in Table 12. As the optimized process parameter setting are different for different characteristics of the composite under consideration. Therefore, to obtain the optimum process parameter setting for optimum response values of all four responses, MRO was carried out using the Grey relation grade method. The multi-response optimization of pultrusion process parameters for four characteristics; UTS, flexural strength, hardness, and % shrinkage of pultruded GFRP composite was carried out by using gray relational grade analysis. The gray relational coefficient corresponding to each process response was computed from normalized raw data. Table 13 reports the normalized values of all four responses and Table 14 give the gray relational grades calculated by averaging the gray relational coefficients corresponding to each process response. Polímeros, 36(2), e20260015, 2026
Optimization of pultruded hybrid bio-filled glass fiber-reinforced composites for lightweight forearm application Table 9. ANOVA for S/N ratio of hardness and % shrinkage. Process parameter
Degree of Freedom (DOF)
Die temp. temperature Pulling speed Hybrid bio filler % Error T
2 2 2 2 8
Sum of square 11.4454 10.3579 17.2845 0.4640 39.5518
Hardness V F-Ratio 5.7227 24.67* 5.1790 22.32* 8.6422 37.25* 0.2320 -
P (%) 28.94 26.19 43.70 1.17 100
Sum of square 7.0894 4.6582 18.1380 0.2329 30.1184
% shrinkage V F-Ratio 3.5447 30.45* 2.3291 20.01* 9.0690 77.91* 0.1164 -
P (%) 23.54 15.47 60.22 0.77 100
*Factors are significant at 95% confidence level; V = Variance; P (%) = % contribution; F-Ratio table = 19 for ANOVA for S/N ratio.
Table 10. ANOVA for raw data of UTS and flexural strength. Process parameter
Degree of Freedom (DOF)
Die temp. Pulling speed Hybrid bio filler % Error T
2 2 2 20 26
UTS Sum of square V 10429.44 5214.72 6655.37 3327.68 24175.89 12087.94 656.82 32.84 41917.53 -
F-Ratio 158.79* 101.33* 368.07* -
P (%) 24.88 15.88 57.67 1.57 100
Flexural strength Sum of square V F-Ratio 15108.69 7554.34 502.37* 5385.73 2692.86 179.08* 7293.44 3646.72 242.51* 300.74 15.03 28088.61 -
P (%) 53.79 19.17 25.97 1.07 100
*Factors are significant at 95% confidence level; V = Variance; P (%) = % contribution; F-Ratio = statistical test value calculated in ANOVA to determine if group means differ significantly.
Table 11. ANOVA for raw data of hardness and % shrinkage. Process parameter Die temp. Pulling speed Hybrid bio filler % Error T
(Degree of Freedom) DOF Sum of square 2 1697.37 2 1471.62 2 3087.87 20 75.50 26 6332.37
Hardness V F-Ratio 848.68 224.82* 735.81 194.92* 1543.93 408.99* 3.77 -
P (%) 26.80 23.24 48.76 1.19 100
Sum of square 3.96 2.44 12.38 0.13 18.93
% shrinkage V F-Ratio 1.983 283.36* 1.224 174.93* 6.192 884.60* 0.007 -
P (%) 20.95 12.93 65.39 0.74 100
*Factors are significant at 95% confidence level; V = Variance; P (%) = % contribution; F-Ratio table = 3.49 for raw data ANOVA.
Table 12. Optimum parameter setting and corresponding response value. Optimized response UTS Flexural strength Hardness % shrinkage
Die temperature Level 3 Level 3 Level 2 Level 2
Parameter setting Pulling speed Level 1 Level 1 Level 2 Level 2
Hybrid bio filler Level 1 Level 2 Level 2 Level 3
Response value at optimum setting 357.56 MPa 350.56 MPa 99 HRK 2.60%
Table 13. Normalized values of responses. Exp. run
Mean UTS
1 2 3 4 5 6 7 8 9
309.84 286.88 208.79 335.85 278.04 305.45 276.52 355.64 307.25
Mean flexural Mean% Normalized Normalized Normalized Normalized % Mean hardness strength shrinkage UTS flexural strength hardness shrinkage 256.91 54.25 5.62 0.69 0.09 0.26 0.00 277.01 79.00 3.58 0.53 0.30 0.72 0.68 248.49 40.25 4.28 0.00 0.00 0.00 0.45 328.83 94.00 3.27 0.87 0.85 1.00 0.79 315.50 78.25 2.64 0.47 0.71 0.71 1.00 261.92 58.50 4.75 0.66 0.14 0.34 0.29 343.35 61.25 3.74 0.46 1.00 0.39 0.63 291.43 72.75 4.61 1.00 0.45 0.60 0.34 315.18 77.50 3.84 0.67 0.70 0.69 0.60
Polímeros, 36(2), e20260015, 2026
9/11
Chandel, R. K., Vaishya, R., Bisht, A. K., Gupta, A., Singh, M. K., & Siengchin, S. Table 14. Grey relational coefficient (∆) and gray relational grade (GRC) with rank for pultruded GFRP Composite. Exp. run ∆ UTS ∆ Flexural strength ∆ hardness ∆ % shrinkage GRC UTS 1 2 3 4 5 6 7 8 9
0.31 0.47 1.00 0.13 0.53 0.34 0.54 0.00 0.33
0.91 0.70 1.00 0.15 0.29 0.86 0.00 0.55 0.30
0.74 0.28 1.00 0.00 0.29 0.66 0.61 0.40 0.31
1.00 0.32 0.55 0.21 0.00 0.71 0.37 0.66 0.40
0.616 0.516 0.333 0.788 0.486 0.594 0.481 1.000 0.603
GRC flexural Strength 0.354 0.417 0.333 0.766 0.630 0.368 1.000 0.477 0.627
GRC hardness 0.403 0.642 0.333 1.000 0.630 0.431 0.451 0.558 0.620
GRC % shrinkage 0.333 0.613 0.476 0.705 1.000 0.413 0.575 0.430 0.555
GCG Rank 0.427 0.547 0.369 0.814 0.687 0.452 0.627 0.616 0.601
8 6 9 1 2 7 3 4 5
Table 15. Mean of Grey Relational Grade at each level for pultruded GFRP Composite. Levels Level 1 Level 2 Level 3 Delta (max-min) Rank
Die temperature (A) 0.448 0.651 0.615 0.203 1
Table 15 represents the result that die temperature has the maximum effect on the multi characteristics of PGFRP followed by hybrid bio filler content and pulling speed in that order. Figure 8 represents that the best combination of pultrusion process parameters for the optimum gray relational grade (optimum characteristics) is the second level of die temperature, the first level of pulling speed, and the second level of % hybrid bio filler for pultruded GFRP composite.
3.1 Confirmation experiment As the optimum parameter setting, second level of die temperature, first level of pulling speed, and second level of hybrid filler was used in the confirmation experiment, the pultruded composite was re-fabricated and tested. The confirmation results showed a tensile strength of 338 MPa, flexural strength of 334.7 MPa, hardness of 92 HRK, and shrinkage of 2.96%, demonstrating good repeatability and validating the effectiveness of the optimized process parameters.
4. Conclusion This study performed single response optimization (SRO) and multi-response optimization (MRO) to determine the optimal pultrusion process parameters affecting the mechanical properties of GFRP composites. The study comprehensively highlights the significant influence of die temperature, pulling speed, and hybrid filler percentage on the mechanical and shrinkage properties of the composite. Optimal values for individual properties varied, with the best UTS obtained at 250 °C die temperature, 100 mm/min pulling speed, and 10% hybrid filler, while the highest flexural strength and hardness were achieved with 15% filler at differing conditions. Shrinkage was minimized at 200 °C, 125 mm/min, and 20% filler. Through Gray Relational Grade (GRG) analysis, the combination of 200 °C, 100 mm/min, and 15% filler emerged as the most effective for overall 10/11
Pulling speed (B) 0.623 0.617 0.474 0.149 3
Hybrid bio filler % (C) 0.498 0.654 0.561 0.156 2
performance enhancement. Among the parameters, hybrid filler content showed the greatest influence on UTS and shrinkage, whereas die temperature had a dominant effect on flexural strength and GRG. Compared to the previous benchmark by Gupta et al.[1], the present work demonstrated notable improvements; UTS by 31%, flexural strength by 6.5%, and hardness by 14.6% with a slight trade-off in shrinkage, which increased marginally from 2.76% to 2.96%. Still conventional polyester-based pultruded GFRP systems typically exhibit shrinkage in the range of 3-6%[8,10]. In comparison, the optimized hybrid bio-filled GFRP composites in this study show lower shrinkage values of 2.96%, indicating improved dimensional stability. This reduction is attributed to enhanced compaction and restricted resin contraction due to the presence of hybrid fillers. The enhanced mechanical strength, dimensional stability, and reduced weight of the optimized hybrid bio-filled GFRP composites make them promising candidates for lightweight forearm protection systems, where high impact resistance and durability are essential for combat and industrial safety applications. The Improvements in tensile strength, flexural strength, hardness, reduced shrinkage, and weight reduction, which represent essential preliminary performance requirements lightweight forearm protection. Comprehensive impact, fatigue, and durability assessments are planned in future work to fully validate the composite for protective applications. These investigations will further validate the applicability of the developed composites for protective and structural applications.
5. Author’s Contribution • Conceptualization – Rajesh Kumar Chandel; Anish Kumar Bisht; Anurag Gupta • Data curation – Rajesh Kumar Chandel; Anish Kumar Bisht Polímeros, 36(2), e20260015, 2026
Optimization of pultruded hybrid bio-filled glass fiber-reinforced composites for lightweight forearm application • Formal analysis – Rajesh Kumar Chandel; Anish Kumar Bisht; Anurag Gupta. • Funding acquisition - Rahul Vaishya • Investigation – Rajesh Kumar Chandel; Anish Kumar Bisht; Anurag Gupta. • Methodology – Rajesh Kumar Chandel; Anish Kumar Bisht • Project administration – Anurag Gupta; Rahul Vaishya; Manoj Kumar Singh. • Resources – Anurag Gupta; Rahul Vaishya • Software – Rajesh Kumar Chandel; Anish Kumar Bisht • Supervision – Rahul Vaishya • Validation – Rajesh Kumar Chandel; Anish Kumar Bisht; Anurag Gupta • Visualization – Rajesh Kumar Chandel; Anish Kumar Bisht; Anurag Gupta. • Writing – original draft – Rajesh Kumar Chandel; Anish Kumar Bisht • Writing – review and editing – Manoj Kumar Singh; Suchart Siengchin
6. References 1. Gupta, A., Vaishya, R., Khan, K. L. A., Walia, R. S., & Singh, H. (2019). Multi-response optimization of the mechanical properties of pultruded glass fiber composite using optimized hybrid filler composition by the gray relation grade analysis. Materials Research Express, 6(12), 125322. https://doi. org/10.1088/2053-1591/ab56f2. 2. Martin, J. (2020). Pultrusion. In E. Miller (Ed.), Plastics products design handbook (pp. 37-74). Boca Raton: CRC Press. https://doi.org/10.1201/9781003064886. 3. Muthukutti, G. P., Singh, M. K., Palaniappan, S. K., Vijayananth, K., Rangappa, S. M., & Siengchin, S. (2026). Valorisation of e-waste CRT glass in polymer composites: sustainable material development and waste reduction. Journal of Material Cycles and Waste Management, 28(1), 570-588. https://doi.org/10.1007/ s10163-025-02439-6. 4. Ye, B. S., Svenson, A. L., & Bank, L. C. (1995). Mass and volume fraction properties of pultruded glass fibre-reinforced composites. Composites, 26(10), 725-731. https://doi. org/10.1016/0010-4361(95)91140-Z. 5. Madenci, E., Özkılıç, Y. O., & Gemi, L. (2020). Experimental and theoretical investigation on flexure performance of pultruded GFRP composite beams with damage analyses. Composite Structures, 242, 112162. https://doi.org/10.1016/j. compstruct.2020.112162. 6. Lackey, E., & Vaughan, J. G. (1994). An analysis of factors affecting pull force for the pultrusion of graphite/epoxy composites. Journal of Reinforced Plastics and Composites, 13(3), 188-198. https://doi.org/10.1177/073168449401300301. 7. Ding, Z., Li, S., & Lee, L. J. (2002). Influence of heat transfer and curing on the quality of pultruded composites. ii: modeling
Polímeros, 36(2), e20260015, 2026
and simulation. Polymer Composites, 23(5), 957-969. https:// doi.org/10.1002/pc.10493. 8. Boukhili, R., Boukehili, H., Daly, H. B., & Gasmi, A. (2006). Physical and mechanical properties of pultruded composites containing fillers and low profile additives. Polymer Composites, 27(1), 71-81. https://doi.org/10.1002/pc.20127. 9. Sathishkumar, T. P., de-Prado-Gil, J., Martínez-García, R., Rajeshkumar, L., Rajeshkumar, G., Rangappa, S. M., Siengchin, S., Alosaimi, A. M., & Hussein, M. A. (2023). Redeemable environmental damage by recycling of industrial discarded and virgin glass fiber mats in hybrid composites: an exploratory investigation. Polymer Composites, 44(1), 318-329. https:// doi.org/10.1002/pc.27047. 10. Ramesh, M., Rajeshkumar, L., Sanjay, M. R., & Siengchin, S. (2025). Sustainable biocomposites based on polylactic acid and agro waste biofillers for lightweight applications: fabrication and properties. Journal of Thermoplastic Composite Materials, 38(10), 3841-3864. https://doi.org/10.1177/08927057251322165. 11. Chandran, A. J., Rangappa, S. M., Suyambulingam, I., & Siengchin, S. (2024). Micro/nano fillers for value‐added polymer composites: a comprehensive review. Journal of Vinyl and Additive Technology, 30(5), 1083-1123. https://doi. org/10.1002/vnl.22106. 12. Shokrieh, M. M., & Aghdami, A. M. (2011). A dynamic transient model to simulate the time dependent pultrusion process of glass/polyester composites. Applied Composite Materials, 18(6), 585-601. https://doi.org/10.1007/s10443-011-9226-7. 13. Bank, L. C. (2006). Composites for construction: structural design with FRP materials. Hoboken: John Wiley & Sons. https://doi.org/10.1002/9780470121429. 14. American Society for Testing and Materials – ASTM. (2010). ASTM D638-10: standard test method for tensile properties of plastics. West Conshohocken: ASTM International. https:// doi.org/10.1520/D0638-10. 15. American Society for Testing and Materials – ASTM. (2007). ASTM D790-07: standard test methods for flexural properties of unreinforced and reinforced plastics and electrical insulating materials. West Conshohocken: ASTM International. https:// doi.org/10.1520/D0790-07. 16. American Society for Testing and Materials – ASTM. (2023). ASTM D785-23: standard test methods for Rockwell hardness of plastics and electrical insulating materials. West Conshohocken: ASTM International. https://doi.org/10.1520/D0785-23. 17. Sylajakumari, P. A., Ramakrishnasamy, R., & Palaniappan, G. (2018). Taguchi grey relational analysis for multi-response optimization of wear in co-continuous composite. Materials, 11(9), 1743. https://doi.org/10.3390/ma11091743. PMid:30223617. 18. Shakya, N., Roux, J. A., & Jeswani, A. L. (2013). Effect of resin viscosity in fiber reinforcement compaction in resin injection pultrusion process. Applied Composite Materials, 20(6), 1173-1193. https://doi.org/10.1007/s10443-013-9320-0. Received: Dec. 08, 2025 Revised: Dec. 25, 2025 Accepted: Dec. 31, 2025 Editor-in-Chief: Sebastião V. Canevarolo.
11/11
ISSN 1678-5169 (Online)
https://doi.org/10.1590/0104-1428.20250093
Research on anti-graffiti coating of nanosilica-modified two-component waterborne polyurethane Qin Li1 , Dingding Xiang2 , Lei Shi3 , Qian Zeng1 , Rui Han4 and Wenhai Lin3* School of Chemical Engineering, Guizhou Institute of Technology, Guiyang, Guizhou Province, China School of Chemistry and Chemical Engineering, Qiannan Normal University for Nationalities, Duyun, Guizhou Province, China 3 Guizhou Zhenhua Qunying Electric Co., Ltd. (State-owned No. 891 Factory), Guiyang, Guizhou Province, China 4 College of Science, Mathematics and Technology, Wenzhou-Kean University, Wenzhou, Zhejiang Province, China 1
2
*linwenhai@whu.edu.cn
Abstract We developed a new type of nano-modified two-component waterborne polyurethane(2K WPU)coating using a regular structure of nano-silica: methyl-polyhedral oligomeric silsesquioxane (POSS) as a modified material. The POSS regular cage structure is used to improve the hardness and wear resistance that waterborne polyurethane lacks, maintain its good water resistance and heat resistance, and does not contain a benzene ring structure in the coating, eliminating the hidden danger of yellowing of the original benzene ring-containing 2K WPU hardening coating. The coating was characterized by Fourier transform infrared spectroscopy, X-ray diffraction, thermogravimetric analysis, scanning electron microscopy, contact angle measurement, UV-visible spectroscopy, water absorption test, hardness test, and anti-graffiti test. The evaluation results show that the modified coating has improved water resistance, hardness and contact angle, has excellent UV resistance, and has excellent anti-graffiti performance. Keywords: anti-graffiti, nanosilica, oligomeric silsesquioxane, surface performance improvement, water-basedpolyurethane. Data Availability: All data supporting the findings of this study are available from the corresponding author upon request. How to cite: Li, Q., Xiang, D., Shi, L., Zeng, Q., Han, R., & Lin, W. (2026). Research on anti-graffiti coating of nanosilica-modified two-component waterborne polyurethane. Polímeros: Ciência e Tecnologia, 36(2), e20260018. https://doi.org/10.1590/0104-1428.20250093
1. Introduction The latest research hotspot in the field of polymer modification is “weak” bond enhancement. The macroscopic properties of polymer networks make it possible to use “weak” bonds to strengthen and toughen covalent polymers[1]. Toughening the network through weak intermolecular interactions, such as ionic bonds, hydrogen bonds, etc., without introducing non-dynamic covalent cross-linkers, the polymer will continue to reorganize or undergo longer time scales or higher temperatures. The exchange of dynamic weak bonds complicates its strengthening and toughening mechanisms and makes them effective in the long term[2]. When encountering the force of scratching or tearing, the weak bonds at the front of the force-propagated crack will preferentially break, thereby alleviating the force of scratching and tearing, which is enough to provide a substantial toughening effect. This opens a new door for us to use nanoparticles containing weak bonds to strengthen polymers, which can be toughened without losing rigidity[3,4]. Water-based two-component polyurethane coatings (2 packs of water-based polyurethane, 2K WPU) have developed
Polímeros, 36(2), e20260018, 2026
rapidly in recent years[5,6]. It generally consists of two parts. One is a hydroxyl-containing water-based resin, in order to increase the solid content, most emulsions are made into 30-50%; the other is hydrophilic modified polyisocyanate, which has good water dispersion properties[7]. The core technology of 2KWPU coating is to utilize the characteristic that the chemical reaction rate between water and polyisocyanate is much lower than the volatilization rate of water[8]. The coating performance of 2KWPU is better than that of single-component products[9], and its applications in indoor and outdoor decoration, high-end metal protective decoration and other fields are booming[10,11]. 2KWPU coatings have extremely low VOC content, good affinity with the substrate surface, strong weather resistance and good waterproofness. They are a representative new generation of high-performance coatings[12-14]. However, the urethane bonds of polyurethane are naturally flexible to a certain extent. This flexibility not only gives it a skin-friendly touch, but also reduces its wear resistance and hardness[15]. The current common method is to add a certain amount of benzene ring structure to the polymer main chain.
1/9
O O O O O O O O O O O O O O O O
Li, Q., Xiang, D., Shi, L., Zeng, Q., Han, R., & Lin, W. But, while improving the wear resistance and hardness, it is also found that under the action of long-term light and heat, the polyurethane coating containing benzene rings will produce yellowing. However, this yellowing is inevitable and physical or chemical methods cannot be used to restore the original color of the coating, which seriously affects the appearance[16]. In recent years, researchers have applied hindered phenolic antioxidant[17], nano cellulose and other modified additives[18], or introduced pentaerythritol tetra (3-mercaptopropionic acid) to hyperbranched the molecular structure[19], which can effectively increase the anti yellowing performance. Cage polyhedral oligomeric silsesquioxane (POSS) is a type of regular nanoparticles, and the general chemical structure is the RnSinO1.5[20]. Its particularity lies in the fact that various functional chemical functional groups can be extended outward from the corners of the cage-like structure. Adjusting the compatibility with different polymers through functional group modification does not affect the cage-like internal structure of silicone. It is a special nanoparticle that has both stability and flexible modification capabilities. POSS is particularly suitable for the preparation of highly consistent nano-modified composite materials[21]. In recent years, as the application of POSS continues to expand, production capacity increases, and prices decrease, it has been extensively studied in the field of nano-modified composite materials as a kind of nano-silica particles with excellent consistency[22,23]. Modified polyurethane materials can be obtained by mixing nano-silica with graphene[24], introducing fluorine-containing groups on the surface of nano-silica[25,26], or using dynamic bonds and modified nano-silica[27]. These materials have enhanced toughness and surface self-cleaning ability while maintaining the flexibility of polyurethane. Previous studies have found that adding POSS with various functional groups to polymers to form hybrid materials can improve hardness, weather resistance, flame retardancy, among others[28,29]. We use methyl POSS with a regular structure as a nano-reinforcement material, combine it with a hydroxylcontaining aqueous emulsion, and finally combine it with a hydrophilic modified polyisocyanate with good water dispersion properties to form a new nano-modified 2K WPU coating, which is highly consistent using POSS. The regular cage structure improves the hardness and wear resistance that water-based polyurethane lacks, and maintains its good water resistance and heat resistance. There is no benzene ring structure in the polymer, eliminating the original 2K WPU hard coating containing benzene rings. There is a hidden danger of yellowing of the layer.
2. Materials and Methods 2.1 Materials Methyl POSS powder was purchased from Wuhan University Silicone New Materials Co., Ltd. Absolute ethanol was reagent grade and purchased from Sinopharm Chemical Reagent Co., Ltd. Deionized water, component A of water-based polyurethane (hydroxyl-containing polyacrylate emulsion: viscosity ≤1500mPa·s, solid content 28.8%, hydroxyl content based on solid content approximately 3.0%) and component B (water-soluble polyisocyanate: Viscosity ≤4500mPa·s, solid content ≥99.8%, NCO content about 22%) is manufactured in our laboratory.
2.2 Preparation of modified composite coating film 2.2.1 Preparation of component A emulsion of nano-modified water-based polyurethane Weigh the hydroxyl-containing polyacrylate emulsion according to the Table 1 and stir it in a 60 °C water bath for 0.5 h. Then weigh a certain amount of methyl POSS according to the Table 1. Mix the methyl POSS and the component A emulsion of the water-based polyurethane, perform high-speed shearing and dispersion for 2 hours, and then filter to obtain the component A emulsion of the nano-modified water-based polyurethane. 2.2.2 Pretreatment of substrate boards Polish the surface of stone and other materials with 400-grit sandpaper, remove floating dust after polishing, and clean the surface with absolute ethanol. The wooden board needs to be polished to remove burrs, then sealed with a laboratory-made primer, and finally sanded with 400-grit sandpaper to remove floating dust. After cleaning the surface of the glass plate with absolute ethanol, it was naturally dried in a dust-free environment. 2.2.3 Preparation of nano-modified water-based polyurethane coating The coating film manufacturing process used to test surface properties is as follows. Weigh the water-soluble polyisocyanate separately according to the formula in Table 1, then weigh the component A emulsion of nano-modified water-based polyurethane according to the formula and add it to the water-soluble polyisocyanate. Stir by hand for 3 minutes until there is no uneven transparent gel. Avoid mixing in air bubbles when stirring. If the viscosity is too high, you can add up to 15% of the total mass of pure water after mixing to adjust the viscosity to 3000-3500 mPa·s.
Table 1. Sample preparation of nano-modified water-based polyurethane coating. Serial Number
n(OH:NCO)
(component B*, g)
(component A*, g)
POSS(g)
pure sample
1:2.5
1
4
0
0.5%POSS
1:2.5
1
4
0.011
2%POSS
1:2.5
1
4
0.044
8%POSS
1:2.5
1
4
0.176
*Component A iswater-based polyurethane emulsion, solid content 28.8wt.%. Component B is water-soluble polyisocyanate, solid content 100wt.%. 0.5% POSS means that POSS accounts for 0.5% of the total mass of solids. 2% and 8% have the same meaning.
2/9
Polímeros, 36(2), e20260018, 2026
Research on anti-graffiti coating of nanosilica-modified two-component waterborne polyurethane Choose a sunny day when the temperature is above 10 °C, and apply two coats of 0.1 kg/m2 on the glass sheet, slate, and wooden board substrate that have been pretreated according to Section 2.2.2, with an interval of 1.5 hours to 2.5 hours. After mixing the two components, use it within 4 hours to ensure stable quality. Dry the painted sample plate at room temperature in a room without dust and air convection. After the coating is cured, maintain it for more than 7 days at a temperature >15 °C and a humidity range of 10%-70% before testing.
2.3 Characterization test 2.3.1 Fourier transform infrared spectroscopy (FTIR) Dry the coating film prepared by the method described in section 2.3.1 for 30min under the infrared light. The infrared spectra of pure sample and nano modified coating film were scanned by the attenuated total reflection method of IRAffinity-1S (Shimadzu, Japan) Fourier transform infrared spectrometer. 2.3.2 Thermogravimetric Analysis (TGA) Coatings prepared according to the method in Section 2.3.1 were cut into approximately 5-10 mg and placed in an Al2O3 crucible. Scans were performed using a Gravimetric Analyzer Q500 (TA, USA) instrument at a heating rate of 10 °C/min and a N flow rate of 50 mL/min in the temperature range from 20 °C to 550 °C.
θ = cos −1
cos θα + cos θγ 2
(1)
Here θα is the advancing contact angle and θγ is the receding contact angle. The final contact angle is the average calculated result after repeating all experiments at least three times. 2.3.6 Substrate adhesion The adhesion of the coating was tested by the crosshatch method, tested according to the standard GB/T92861998, using a 5120 cross-hatch tester (BYK Chemical) to prepare a coated glass sheet sample according to the method described in Section 2.2.3. Use professional tools to draw grids and use special tape to peel. GB/T9286-1998 divides the adhesion of the tested items into 6 levels, including levels 0, 1, 2, 3, 4, and 5 according to the adhesion from large to small. Level 0 indicates that the coating cut edges are completely smooth, with no peeling.Level 4 indicates that large fragments of the coating peel off at the cut edges, or some squares partially or completely peel off. The affected cross-cut area is significantly greater than 35%, but not significantly greater than 65%. Level 5 indicates that the degree of peeling exceeds that of Level 4. 2.3.7 Hardness
The coating prepared according to the method described in Section 2.3.1 was broken off under liquid nitrogen cooling, and then its surface and cross-section were coated with a thin layer of gold. The surface/section morphology and element distribution of the pure sample and the nano-modified coating were examined by using a SU8010 (Hitachi, Japan) scanning electron microscope.
The hardness test of the coating is based on “GB/ T6739-2006 Pencil Method for Determination of Paint Film Hardness of Medium Color Paints and Varnishes” as the standard, using a PPH pencil hardness tester (Shanghai Modern Environment) using pencils of different hardness at a certain speed according to Section 2.3. Immediately after the tip of the pencil touches the coating, push the test plate at a speed of 0.5mm/s-1mm/s towards the direction away from the operator for a distance of at least 7mm. The hardness of the paint film can be determined by scratching a sample of a glass plate coated by the method described in Section 2 to produce traces.
2.3.4 Ultraviolet-Visible Spectroscopy (UV-VIS)
2.3.8 Anti-graffiti
2.3.3 Scanning electron microscope (SEM)
The UV-visible spectrophotometric test of the coating is to use the coating film prepared by the method described in Section 2.3.1, using a UV-2600 UV-visible spectrophotometer (Shimadzu, Japan), setting the wavelength to 200-700nm, to study under the irradiation of ultraviolet-visible light in this range, the material absorbs or transmits ultraviolet-visible light, and its transparency and transmittance in the visible light range are explored through absorbance and transmittance. 2.3.5 Contact angle test Brush the cured pure sample and nano-modified coating on the glass sheet, slate, and wooden board substrate prepared according to the method in Section 2.2.3, and use an OCA 15EC instrument with a drip angle observation system (German Dataphysics Company), the relative hydrophilicity of the surface was measured by measuring the static contact angle of 5 μL H2O on the surface of each film using the static sessile drop method. The films to be tested were vacuum dried before testing. The measurement time was set to less than 10 seconds (stabilization time from droplet droplet initiation to measurement) to reduce the effect of water evaporation. The contact angle θ is calculated using Equation 1[30]: Polímeros, 36(2), e20260018, 2026
Brush the cured pure sample and nano-modified coating on the glass sheet prepared according to the method in Section 2.2.3. A simple anti graffiti test was carried out using the marking method. Mark the surface of the sample with the coating film on the glass graffiti simulation plate using a water-based marker (Baoke MP2906, including black, red, and blue water-based inks) and an oil-based marker (Baoke MP2916, including black, red, and blue oil-based inks). After 24 hours, scrub with water, then scrub with 99% alcohol and take photos to record the experimental results.
3 Results and Discussions 3.1 Characterization of peeled coating films 3.1.1 FTIR analysis The infrared spectrum layer of pure sample and nanomodified coatingare shown in Figure 1. In the infrared spectrum of the pure sample, the broad peak near 3300 cm-1 is the stretching vibration peak of the N-H group, and the peak near 1735 cm-1 is the stretching vibration peak of the C=O bond. The bending vibration peak near 1650 cm-1 3/9
Li, Q., Xiang, D., Shi, L., Zeng, Q., Han, R., & Lin, W. is the bending vibration peak of N-H, and the peak near 1400 cm-1 is the stretching vibration peak of C-N bond, but there is no ester bond near 1730 cm-1[31]. It can be seen from the infrared spectrum of the Nano-modified coating that as the POSS content increases, the peak at 1110 cm-1 is the stretching vibration peak of Si-O-Si, and the peak at 780 cm-1. The stretching vibration peak is the stretching vibration peak of Si-C. The bending vibration peaks of in-plane and out-of-plane C-H are at 1410, 970, 1275 and 1000 cm-1. The skeleton vibration peaks of Si-O-Si are located at 475 and 812 cm-1[13]. As the proportion of POSS in the mixed active layer increases, the gap between the peak height of Si-O-Si and the peak height of C-N bond and C=O bond gradually narrows, proving that the POSS content in the coating film has increased[32]. 3.1.2 TGA The Figure 2 shows that the nano-modified coating after POSS modification decomposes faster than the pure polyurethane before modification. A trace amount of POSS powder has a greater impact on the crystal structure.
The less POSS is added, the faster it decomposes. However, the final thermal decomposition residual amount results show that the more POSS powder is added, the greater the residual amount. This is because although POSS interferes with the crystallization of polyurethane and accelerates the thermal decomposition of the polyurethane polymer chain, the cage structure of POSS itself determines its higher thermal decomposition temperature. As POSS increases, the final residual amount increases[33]. At the same time, too much POSS also affects the thermal decomposition of polyurethane polymers. It is proved that a trace amount of POSS will accelerate the thermal decomposition of polyurethane. 3.1.3 SEM analysis As can be seen from the sample cross-section Figure 3, the pure sample coating forms a layered scaly structure. As the proportion of POSS added in the nano-modified coating increases, more and more round POSS particles appear in the layer. Similar structures are relatively evenly distributed among themselves and embedded in the polyurethane coating. At the same time, when we used SEM surface scanning for element content, we observed an interesting phenomenon: silicon elements tend to be enriched on the surface of the coating film (Table 2). As the addition ratio of POSS powder increases, the silicon content in the top layer becomes higher and higher, and the gap between the silicon content in the bottom layer and the silicon content in the bottom layer becomes wider and wider. This tendency of POSS to be enriched on the surface is conducive to the effective enhancement of surface properties. 3.1.4 UV-VIS analysis
Figure 1. Infrared absorption spectra of films with different POSS modification ratios.
It can be seen from the Figure 4 that as the proportion of POSS is gradually increased, the UV-visible light transmittance of the composite coating gradually decreases. It is consistent with the test results in 3.1.1 and 3.1.4. The addition of POSS destroys the regular crystalline structure of the original polyurethane, and the transparency of the composite coating can be seen by naked eyes. Microscopically, there will be more diffuse reflection and refraction of light in the coating, which consumes energy and significantly reduces the transmittance.Only adding 0.5w.t% POSS can significantly reduce the UV-visible light transmittance of the coating[34,35].
Figure 2. TGA comparison of coating films with or without POSS added. 4/9
Polímeros, 36(2), e20260018, 2026
Research on anti-graffiti coating of nanosilica-modified two-component waterborne polyurethane Table 2. Upper and bottom surface element contents of coating films with different POSS contents. Upper surface
Group pure Sample 0.5%POSS 2%POSS 8%POSS
C 74.09 68.59 77.68 61.10
Bottom surface Si
0.04 7.74 9.57 11.28
C 73.05 67.16 68.08 68.05
Si 0.11 3.64 1.83 4.22
Figure 3. SEM comparison of coating films with or without POSS added (A\B\C\D represent pure sample / 0.5%POSS / 2%POSS / 8%POSS, respectively).
The pass rate makes the composite coating promising as an efficient anti-UV material.
3.2 Coating surface performance characterization 3.2.1 Contact angle analysis The contact angle of the nano-modified composite coating on the surface of the glass sheet and the stone surface after adding POSS powder is larger than that of the pure sample coating before modification in Figure 5 and Figure 6. By adding POSS to the coating, the contact angle increases from approximately 85º in glass and 87º in stone to near or above 100º, achieving hydrophobic behavior on the surface. This is related to the literature reporting that POSS, as a hydrophobic organic silicon nanoparticle, is good at surface enrichment. When POSS is added to the coating, it changes the surface polarity, making the coating more hydrophobic[36,37].However, as the amount of POSS powder added reaches 8w.t%, the contact angle decreases. Polímeros, 36(2), e20260018, 2026
Figure 4. UV-VIS comparison of coating films with or without POSS added. 5/9
Li, Q., Xiang, D., Shi, L., Zeng, Q., Han, R., & Lin, W. This reduction in contact angle may be due to localized aggregation caused by excessive POSS addition. Only 0.5w.t% POSS is needed to effectively increase the contact angle of the coating by 10º-15º, proving that POSS, as a nanomodifier, is highly efficient in improving surface properties. 3.2.2 Substrate adhesion and hardness analysis It can be seen from Table 3 that the adhesion of the nano-modified composite coating on the glass surface is significantly improved after adding POSS powder. This may
be because POSS has Si-O-Si bonds and has a tendency of surface enrichment in SEM tests. Therefore, it is consistent with the surface affinity of the glass piece will be stronger. As spherical nanoparticles with a regular cage structure, POSS also significantly improves the surface hardness of the polyurethane coating. Ghermezcheshme et al.’s study also showed thatintrinsic hardness of POSS affected the crosslink density, the result of which was affected free volumeand improved scratch resistance of POSS/2K WPU hybrid coatings[38,39]. An 8w.t% addition of POSS can increase the hardness of the 2K WPU coating on the glass substrate from 2H to 6H. 3.2.3 Analysis of anti-graffiti capabilities
Figure 5. Contact angle of coating film on glass surface.
As can be seen from Figure 7, through the experiment of simulating graffiti and then cleaning, it was found that the graffiti marks drawn with water-based markers can be easily removed with ordinary water, while the marks drawn with oil-based markers will only fade slightly. Wait until the graffiti simulation plate is dry and then wipe it with 99% alcohol. The traces of the oil-based marker are completely removed. This proves that the nano-modified composite coating also has strong anti-graffiti ability. The key to preventing graffiti is that graffiti contaminant cannot penetrate into the coating or even the substrate itself. When erasing graffiti, the binding energy between the cleaning agent and the pollutant is greater than the binding energy between the pollutant and the coating surface[40-42]. The polarity of graffiti contaminant in water-based marking is stronger, and the binding energy with water is stronger, so they can be completely removed by water[43-45]. When cleaning graffiti traces in oil-based marking with water, it will only fade slightly, because graffiti traces in oil-based marking are more non-polar and have lower binding energy with water, which is not enough to overcome their
Table 3. Substrate adhesion and hardness of coating films with different POSS contents.
Figure 6. Contact angle of coating film on stone surface.
Group pure sample 0.5% POSS 2%POSS 8%POSS
Adhesion level (glass surface) 3 0 0 0
hardness grade 2H 4H 4H 6H
Figure 7. Comparison chart of erasing graffiti effects. (a) After graffiti, (b) wiped by water, (c) wiped by 99% alcohol. 6/9
Polímeros, 36(2), e20260018, 2026
Research on anti-graffiti coating of nanosilica-modified two-component waterborne polyurethane binding energy with the coating surface. The graffiti marks drawn by oil-based markers can be erased by 99% alcohol, proving that the binding energy between 99% alcohol and graffiti marks drawn by oil-based markers can overcome its binding energy with the coating surface. At the same time, it also proves the effectiveness of our coating in resisting graffiti. These graffiti contaminant cannot penetrate into the interior of the coating, but only adhere to the coating surface. This may be because the layer-by-layer scale-like structure prevents the penetration of graffiti by water-based markers and oil-based markers (see the electron microscope picture), proving that the nano-modified composite coating also has strong anti-graffiti capabilities. The coating also has good application prospects as an anti-graffiti coating.
4. Conclusions Methyl POSS with a regular structure is used as a nano-reinforcement material, combined with a hydroxylcontaining aqueous emulsion, and finally combined with a hydrophilic modified polyisocyanate with good water dispersion properties to form a new nano-modified 2K WPU coating. This new polyurethane hybrid coating has excellent yellowing resistance due to the absence of benzene ring in the main chain.The SEM image proves that the spherical structure of POSS is still perfectly preserved. At the same time, when scanning the element content, it is observed that the silicon element is enriched towards the surface of the coating film. Adhesion and hardness experiments support this: hardness and adhesion also increase with the addition of POSS. The adhesion of the nano-modified composite coating on the surface of the glass sheet after adding POSS powder was significantly improved. Through the water absorption experiment, it was discovered that when the appropriate proportion of POSS nanoparticles was added, the water absorption peak value would change with temperature changes. Through contact angle experiments, it was found that the contact angle of the nano-modified composite coating on the surface of glass, stone, and wood after adding POSS powder is larger than before without adding POSS powder. Only 0.5w.t% POSS is needed to effectively improve the coating 10º-15º of contact angle, proving that POSS can be used as an efficient nano-modifier to improve surface properties. The research results also show that only adding 0.5w.t% POSS can significantly reduce the UV-visible light transmittance of the coating film, which makes the composite coating promising as an efficient anti-UV material. The anti-graffiti ability experiment also proved that the nano-modified composite coating can also have good application prospects as an anti-graffiti coating. Water-based graffiti marks and contaminant can be completely removed by water. When cleaning oil-based graffiti marks with water, due to its stronger non-polar nature and lower binding energy with water, it is not enough to overcome its binding energy with the coating surface. Therefore, simply scrubbing with water cannot completely remove it. However, oil-based graffiti marks can be erased by 99% of alcohol, proving that the binding energy between 99% of alcohol and oil-based graffiti marks can overcome its binding energy with the coating surface. At the same time, it also proves that both water-based and oil-based graffiti contaminant Polímeros, 36(2), e20260018, 2026
cannot penetrate into the interior of the coating, but only adhere to the coating surface. This new type of composite water-based coating has anti-graffiti, anti-yellowing, and long-term weathering resistance, making it very suitable for outdoor cultural relics and public infrastructure.
5. Author’s Contribution • Conceptualization – Qin Li; Dingding Xiang; Lei Shi; Qian Zeng; Rui Han; Wenhai Lin. • Data curation – Qin Li; Lei Shi; Wenhai Lin. • Formal analysis – Qin Li; Lei Shi. • Funding acquisition – Qin Li; Dingding Xiang. • Investigation – Qin Li; Qian Zeng. • Methodology – Qin Li; Wenhai Lin. • Project administration – Wenhai Lin. • Resources – Qin Li; Dingding Xiang. • Software – NA. • Supervision – NA. • Validation – Dingding Xiang; Qian Zeng; RuiHan. • Visualization – Dingding Xiang. • Writing – original draft – Qin Li; Dingding Xiang; Lei Shi. • Writing – review & editing – Lei Shi; Rui Han.
6. Acknowledgements Supported by Guizhou Provincial Basic Research Program(Natural Science) (Qiankeheji-ZK [2024] General517). Guizhou Institute of Technology High-level Talent Scientific Research Fund Launch Project (2023GCC022).The Young Scientific and Technological Talents Growth Project of Department of Education of Guizhou Province (Qianjiaohe KY [2022] 353). Project of Education Department of Guizhou Province (Grant No KY [2014]214). The Teaching Reform Research Project of Guizhou Institute of Technology (2022TDFJG04). Guizhou Institute of Technology High-level Talent Scientific Research Fund Launch Project (2023GCC026).
7. References 1. Wang, S., Hu, Y., Kouznetsova, T. B., Sapir, L., Chen, D., HerzogArbeitman, A., Johnson, J. A., Rubinstein, M., & Craig, S. L. (2023). Facile mechano chemical cycloreversion of polymer cross-linkers enhances tear resistance. Science, 380(6651), 12481252. https://doi.org/10.1126/science.adg3229. PMid:37347867. 2. Zhang, J., Chang, Y., Jin, S., Yang, H., Chen, S., Zhang, W., & Chen, Y. (2023). Study on the preparation and performance of SiC nanoparticle reinforced polyurethane coatings. Journal of Applied Polymer Science, 140(30), e54096. https://doi. org/10.1002/app.54096. 3. Meng, X., Qiao, Y., Do, C., Bras, W., He, C., Ke, Y., Russell, T. P., & Qiu, D. (2022). Hysteresis-free nanoparticle-reinforced hydrogels. Advanced Materials, 34(7), 2108243. https://doi. org/10.1002/adma.202108243. PMid:34837255. 4. Singh, R. K., Gangwar, S., & Singh, D. K. (2023). Experimental analysis with GRA-PCA-based hybrid optimization to analyze the effect of hydroxyapatite nanoparticle-reinforced UHMWPE for hip joint. Journal of Advanced Manufacturing Systems, 22(02), 423-444. https://doi.org/10.1142/S021968672350021X. 7/9
Li, Q., Xiang, D., Shi, L., Zeng, Q., Han, R., & Lin, W. 5. Yin, X., Pang, H., Luo, Y., & Zhang, B. (2021). Eco-friendly functional two-component flame-retardant waterborne polyurethane coatings: a review. Polymer Chemistry, 12(38), 5400-5411. https://doi.org/10.1039/D1PY00920F. 6. Wei, Z., Liu, Z., Fu, X., Wang, Y., Yuan, A., & Lei, J. (2021). Effect of crystalline structure on water resistance of waterborne polyurethane. European Polymer Journal, 157(2), 110647. https://doi.org/10.1016/j.eurpolymj.2021.110647. 7. Peng, Z., Tang, L., Yuan, Y., & Qu, J. (2020). Synthesis and properties of water-dispersible polyisocyanates carrying sulfonate. Journal of Coatings Technology and Research, 17(2), 345-359. https://doi.org/10.1007/s11998-019-00277-4. 8. Gong, C., Xiao, B., Hu, X., Xian, Y., Wang, P., Yang, Y., Luo, X., Li, M., Liu, J., Ding, Y., Xu, P., & Liu, C. (2022). A waterborne polyurethane-based hybrid fluorescent silicon quantum dot. Journal of Applied Polymer Science, 139(35), e52824. https://doi.org/10.1002/app.52824. 9. Mumtaz, F., Zuber, M., Zia, K. M., Jamil, T., & Hussain, R. (2013). Synthesis and properties of aqueous polyurethane dispersions: influence of molec-ular weight of polyethylene glycol. Korean Journal of Chemical Engineering, 30(12), 2259-2263. https://doi.org/10.1007/s11814-013-0166-9. 10. Dall Agnol, L., Dias, F. T. G., Ornaghi, H. L., Jr., Sangermano, M., & Bianchi, O. (2021). UV-curable waterborne polyurethane coatings: A state of the art and recent advances review. Progress in Organic Coatings, 154, 106156. https://doi.org/10.1016/j. porgcoat.2021.106156. 11. Xu, X., Zhou, Z., Qin, L., Yu, C., & Zhang, F. (2022). Preparation of PVA/PU/PUA microcapsules and application in self-healing two-component waterborne polyurethane coatings. Journal of Coatings Technology and Research, 19(3), 977-988. https:// doi.org/10.1007/s11998-021-00577-8. 12. Guo, L., Huang, S., & Qu, J. (2018). Synthesis and properties of high-func-tionality hydroxyl-terminated polyurethane dispersions. Progress in Organic Coatings, 119, 214-220. https://doi.org/10.1016/j.porgcoat.2018.02.033. 13. Sheng, Y., Wang, M., Zhang, K., Wu, Z., Chen, Y., & Lu, X. (2021). An “inner soft external hard”, scratch-resistant, selfhealing waterborne poly(urethane-urea) coating based on gradient metal coordination structure. Chemical Engineering Journal, 426, 131883. https://doi.org/10.1016/j.cej.2021.131883. 14. Xia, P., Liu, P., Wu, S., Zhang, Q., Wang, P., Hu, R., Xing, K., Liu, C., Song, A., Yang, X., & Huang, Y. (2022). Highly stretchable and sensitive flexible resistive strain sensor based on waterborne polyurethane polymer for wearable electronics. Composites Science and Technology, 221, 109355. https://doi. org/10.1016/j.compscitech.2022.109355. 15. Fazeli, M., Liu, X., & Rudd, C. (2022). The effect of waterborne polyurethane coating on the mechanical properties of epoxy-based composite containing recycled carbon fibres. Surfaces and Interfaces, 29, 101684. https://doi.org/10.1016/j. surfin.2021.101684. 16. Malik, M., & Kaur, R. (2018). Influence of aliphatic and aromatic isocyanates on the properties of poly(ether ester) polyol based PU adhesive system. Polymer Engineering and Science, 58(1), 112-117. https://doi.org/10.1002/pen.24537. 17. Li, J., Han, X., Huyan, C., Liu, D., Li, X., Li, H., & Chen, F. (2023). Hindered phenolic antioxidant modified waterborne polyurethane films with excellent thermal stability and anti-aging performance at high temperature. Progress in Organic Coatings, 176, 107398. https://doi.org/10.1016/j.porgcoat.2022.107398. 18. Zhang, H., She, Y., Zheng, X., Chen, H.-Y., & Pu, J.-W. (2014). Optical and mechanical properties of polyurethane/ surface-modified nanocrystalline cellulose composites. Chinese Journal of Polymer Science, 32(10), 1363-1372. https://doi. org/10.1007/s10118-014-1526-6. 8/9
19. Fu, J., Yu, H., Wang, L., Lin, L., & Khan, R. U. (2020). Preparation and properties of UV-curable hyperbranched polyurethane acrylate hard coatings. Progress in Organic Coatings, 144, 105635. https://doi.org/10.1016/j.porgcoat.2020.105635. 20. Huang, P.-H., Laakso, M., Edinger, P., Hartwig, O., Duesberg, G. S., Lai, L.-L., Mayer, J., Nyman, J., Errando-Herranz, C., Stemme, G., Gylfason, K. B., & Niklaus, F. (2023). Threedimensional printing of silica glass with sub-micrometer resolution. Nature Communications, 14(1), 3305. https://doi. org/10.1038/s41467-023-38996-3. PMid:37280208. 21. Bauer, J., Crook, C., & Baldacchini, T. (2023). A sinterless, low-temperature route to 3D print nanoscale optical-grade glass. Science, 380(6648), 960-966. https://doi.org/10.1126/ science.abq3037. PMid:37262172. 22. Zhang, W., Zhuang, X., Li, X., Lin, Y., Bai, J., & Chen, Y. (2009). Preparation and characterization of organic/inorganic hybrid polymers containing polyhedral oligomeric silsesquioxane via RAFT polymerization. Reactive & Functional Polymers, 69(2), 124-129. https://doi.org/10.1016/j.reactfunctpolym.2008.11.009. 23. Liu, Y., Zeng, K., & Zheng, S. (2007). Organic-inorganic hybrid nanocomposites involving novolac resin and polyhedral oligomeric silsesquioxane. Reactive & Functional Polymers, 67(7), 627635. https://doi.org/10.1016/j.reactfunctpolym.2007.04.002. 24. Chen, K., Liu, H., Zhou, J., Sun, Y., & Yu, K. (2022). Polyurethane blended with silica-nanoparticle-modified graphene as a flexible and superhydrophobic conductive coating with a self-healing ability for sensing applications. ACS Applied Nano Materials, 5(1), 615625. https://doi.org/10.1021/acsanm.1c03414. PMid:35128341. 25. Fu, P., Ou, J., He, Y., Hu, Y., Wang, F., Fang, X., Li, W., & Amirfazli, A. (2024). Robust superhydrophobic coating with carbon nanotubes and silica nanoparticles in the matrix of fluorinated polyurethane. Surfaces and Interfaces, 45, 103890. https://doi.org/10.1016/j.surfin.2024.103890. 26. Jie, L., Nan, Z., Zonglin, L., Ze, L., Guoqing, W., Lishuang, G., & Jing, L. (2022). Fast self-healing and antifouling polyurethane/ fluorinated polysiloxane-microcapsules-silica composite material. Advanced Composites and Hybrid Materials, 5(3), 1899-1909. https://doi.org/10.1007/s42114-022-00515-1. 27. Yanan, Z., Yeming, S., Minhui, W., & Xun, L. (2022). UVcurable self-healing, high hardness and transparent polyurethane acrylate coating based on dynamic bonds and modified nanosilica. Progress in Organic Coatings, 172, 107051. https://doi. org/10.1016/j.porgcoat.2022.107051. 28. Chen, D., Yi, S., Wu, W., Zhong, Y., Liao, J., Huang, C., & Shi, W. (2010). Synthesis and characterization of novel room temperature vulcanized (RTV) silicone rubbers using VinylPOSS derivatives as cross linking agents. Polymer, 51(17), 3867-3878. https://doi.org/10.1016/j.polymer.2010.06.028. 29. Chen, D., Nie, J., Yi, S., Wu, W., Zhong, Y., Liao, J., & Huang, C. (2010). Thermal behaviour and mechanical properties of novel RTV silicone rubbers using divinyl-hexa[(trimethoxysilyl)ethyl]POSS as cross-linker. Polymer Degradation & Stability, 95(4), 618-626. https://doi.org/10.1016/j.polymdegradstab.2009.12.002. 30. Uragami, T., Tsukamoto, K., Inui, K., & Miyata, T. (1998). Pervaporation characteristics of a benzoyl chitosan membrane for benzene-cyclohexane mixtures. Macromolecular Chemistry and Physics, 199(1), 49-54. https://doi.org/10.1002/(SICI)15213935(19980101)199:1<49::AID-MACP49>3.0.CO;2-B. 31. Anand, A., Jirimali, H. D., Kulkarni, R. D., & Gite, V. (2018). Utilisation of sebacic acid and nanohydroxyapatite in polyurethane nanocomposite coating. Green Materials, 6(2), 65-75. https://doi.org/10.1680/jgrma.17.00028. 32. Lin, W., Liu, Z., Li, Q., Rong, Q., Zu, H., & Sang, M. (2020). Dehydration of caprolactam–water mixtures by composite membranes with nano silica/polyacrylate active layer by emulsion polymerization. Desalination and Water Treatment, 208, 125-135. https://doi.org/10.5004/dwt.2020.26464. Polímeros, 36(2), e20260018, 2026
Research on anti-graffiti coating of nanosilica-modified two-component waterborne polyurethane 33. Qin, L., Chuanwen, L., Dingding, X., & Dongzhi, C. (2021). Separation of green solvent dimethyl carbonate/methanol azeotropic mixture by pervaporation with polydimethylsiloxane/polyhedral oligomeric silsesquioxane composite membrane. Global NEST Journal, 23(3), 458-467. https://doi.org/10.30955/gnj.003512. 34. Kang, J.-M., Cho, H.-J., Lee, J., Lee, J.-I., Lee, S.-K., Cho, N.-S., Hwang, D.-H., & Shim, H.-K. (2006). Highly bright and efficient electroluminescence of new PPV derivatives containing polyhedral oligomeric silsesquioxanes (POSS) and their bends. Macromolecules, 39(15), 4999-5008. https://doi. org/10.1021/ma0603377. 35. Wahab, M. A., Mya, K. Y., & He, C. (2010). Synthesis, morphology, and properties of hydroxyl terminated-POSS/ polyimide low-k nanocomposite films. Journal of Polymer Science. Part A, Polymer Chemistry, 46(17), 5887-5896. https://doi.org/10.1002/pola.22906. 36. Zhao, H., She, W., Shi, D., Wu, W., Zhang, Q.-C., & Li, R. K. Y. (2019). Polyurethane/POSS nanocomposites for superior hydrophobicity and high ductility. Composites. Part B, Engineering, 177, 107441. https://doi.org/10.1016/j.compositesb.2019.107441. 37. Wang, X., Chen, G.-X., Han, R., Zhou, Z., & Li, Q. (2024). Controlled synthesis of non-functionalized POSS nanoparticles with hydrophobic to hydrophilic wettability transition. Progress in Organic Coatings, 191, 108398. https://doi.org/10.1016/j. porgcoat.2024.108398. 38. Prządka, D., Marcinkowska, A., & Andrzejewska, E. (2016). POSS-modified UV-curable coatings with improved scratch hardness and hydrophobicity. Progress in Organic Coatings, 100, 165-172. https://doi.org/10.1016/j.porgcoat.2016.01.011. 39. Ghermezcheshme, H., Mohseni, M., & Yahyaei, H. (2015). Use of nanoindentaion and nanoscratch experiments to reveal the mechanical behavior of POSS containing polyurethane nanocomposite coatings: the role of functionality. Tribology International, 88, 66-75. https://doi.org/10.1016/j.triboint.2015.02.023.
Polímeros, 36(2), e20260018, 2026
40. Adapala, P., Gaur, S., Puri, R. G., & Khanna, A. S. (2015). Development and evaluation of nano-silica dispersed polyurethane based coatings for improved anti-graffiti and scratch resistance. Open Journal of Applied Sciences, 5(12), 808-818. https://doi.org/10.4236/ojapps.2015.512077. 41. Mariateresa, L., & Maurizio, M. (2014). Surface characterization and effectiveness evaluation of anti-graffiti coatings on highly porous stone materials. Applied Surface Science, 288, 466-477. https://doi.org/10.1016/j.apsusc.2013.10.056. 42. Rossi, S., Deflorian, F., & Fedel, M. (2019). Polysilazane-based coatings: corrosion protection and anti-graffiti properties. Surface Engineering, 35(4), 343-350. https://doi.org/10.108 0/02670844.2018.1465748. 43. Rabea, A. M., Mirabedini, S. M., & Mohseni, M. (2012). Investigating the surface properties of polyurethane based anti-graffiti coatings against UV exposure. Journal of Applied Polymer Science, 124(4), 3082-3091. https://doi.org/10.1002/ app.35344. 44. Rabea, A. M., Mohseni, M., Mirabedini, S. M., & Hashemi Tabatabaei, M. (2012). Surface analysis and anti-graffiti behavior of a weathered polyurethane-based coating embedded with hydrophobic nano silica. Applied Surface Science, 258(10), 4391-4396. https://doi.org/10.1016/j.apsusc.2011.12.123. 45. Amrutkar, S., More, A., Mestry, S., & Mhaske, S. T. (2022). Recent developments in the anti-graffiti coatings: an attentive review. Journal of Coatings Technology and Research, 19(3), 717-739. https://doi.org/10.1007/s11998-021-00580-z. Received: Dec. 04, 2025 Revised: Feb. 03, 2026 Accepted: Feb. 04, 2026 Associate Editor: José A. C. G. Covas
9/9
ISSN 1678-5169 (Online)
https://doi.org/10.1590/0104-1428.20250104
Surface-modified Agave vilmoriniana fibers for enhanced thermo-mechanical and interfacial performance in composites Gowtham Saravanan1* and Ramakrishnan Thirumalaisamy1 Centre for Advanced Materials & Testing, Department of Mechanical Engineering, Sri Eshwar College of Engineering, Coimbatore, Tamil Nadu, India
1
*gowtham.s@sece.ac.in
Abstract This study examines Agave vilmoriniana leaf fibers after consecutive alkali, silane, and starch treatments for polymer composites. The treatments reduces hemicellulose, moisture absorption and improving fiber stability. X-ray diffraction Analysis showed intensified (002) peaks that confirming improved crystalline ordering, while Fourier Transform Infrared spectra showed the reduction of hemicellulose and lignin and after alkali and silane treatments by the peaks around 1730cm−1 band and the peak 750cm−1 confirms the emergence of siloxane linkages. Subsequently, thermal analysis using Thermogravimetry showed improved thermal stability with onset and maximum degradation temperatures were rising from ~285 to 305 °C and ~340 to 355 °C respectively. Mechanical testing shows starch coating increases stiffness to 23.42 GPa. Scanning Electron Microscopic image observations confirmed the gradual surface modifications. The result makes that the fibers were more suitable for high-performance, moisture-resistant and polymer composites. Keywords: Agave vilmoriniana leaf fibers, alkali treatment, silane coupling, starch coating, mechanical properties. Data Availability: All data supporting the findings of this study are available from the corresponding author upon request. How to cite: Saravanan, G., & Thirumalaisamy, R. (2026). Surface-modified Agave vilmoriniana fibers for enhanced thermo-mechanical and interfacial performance in composites. Polímeros: Ciência e Tecnologia, 36(2), e20260020. https://doi.org/10.1590/0104-1428.20250104.
1. Introduction Global usage of fiber-reinforced composite’s continues to gradually expanding which driven by their elevated strength-to-weight ratio, corrosion resistivity and design versatility. Traditionally, alternative synthetic fibers took over the market which were accounting for more than 90% of the 12 million tonnes of fiber reinforcements produced annually worldwide. While these materials deliver excellent mechanical performance, their production is energy-intensive, non-biodegradable, and heavily reliant on petrochemical resources, leading to significant environmental concerns. For example, the carbon footprint of glass fiber production can exceed 1.5 kg CO2 per one kilo fiber and end-of-life disposal often results in landfill accumulation or incineration. Alternatively, natural fiber were renewable, biodegradable, lightweight, and often created with far reduced energy inputs. Recent life-cycle studies show that natural fiber composites can cut energy use during production by up to 60% and greenhouse gas emissions by more than 50% compared to synthetic composites. To meet the European Union’s End-of-Life Vehicle Directive (2000/53/EC), which requires 95% material recovery and recyclability, the European automotive industry has already used natural fiber composites in door panels, dashboards, and interior trims[1-4]. Natural fibers are good for the environment in some ways, but they also have some fundamental issues that make them hard to utilize in high-performance applications.
Polímeros, 36(2), e20260020, 2026
Because they had a lot of cellulose and hemicellulose in them, they were hydrophilic, which meant they held too much water, swelled, and loss of dimensional stability. These challenges are particularly evident in Agave vilmoriniana fibers, which represent a promising yet underexplored reinforcement material. However, their high lignin content and the presence of surface impurities restrict effective compatibility with polymer matrices[5,6]. Natural fibers are inherently hydrophilic because of abundance of hydroxyl groups in their composition structure. This characteristic adversely affects dimensional stability and weakens fiber–matrix adhesion. Moisture uptake leads to fiber-swelling, the development of internal stresses, and the formation of interfacial microcracks, thereby reducing the efficiency of stress transfer[7-9]. The polarity mismatch between fibers-matrices pave the way to poor wettability, low resin impregnation, and void formation. These defects act as sites of stress concentration and adversely affect the tensile, flexural, and fatigue performance of composite materials[8,10,11]. Repeated cycles of moisture absorption and desorption accelerate interfacial debonding and degradation, leading to a progressive reduction in material durability. To address these limitations, surface treatments such as alkali treatment, silane modification, and starch coating have been extensively investigated to reduce hydrophilicity and enhance fiber–matrix compatibility[12,13].
1/9
O O O O O O O O O O O O O O O O
Saravanan, G., & Thirumalaisamy, R. These modifications enhance interfacial adhesion by reducing polarity and promoting chemical interaction with the matrix. However excessive treatment can modify the fiber structure or compromise environmental sustainability. The primary challenge lies in developing treatment strategies that achieve improved interfacial adhesion while preserving the inherent environmental benefits of natural fibers[14,15]. Agave vilmoriniana leaf fiber (AVLF) has get attention as a promising plant based natural reinforcement owing to its higher tensile strength, lower density, and renewable origin. Although several studies have reported the influence of alkali treatment on the mechanical performance of Agave derived fibers, investigations specifically focused on Agave vilmoriniana remain limited[16,17]. The combined impact of multi-treatments such as alkali treatment, silane functionalization, and starch coating has not been explored in detail. Some studies have indicated that treating Agave fibers with alkali solutions followed by silane agents improves mechanical properties and fiber–matrix adhesion[18,19]. However, a complete analysis of the synergistic effects of these treatments for Agave vilmoriniana is yet to be reported. This research gap offers the potential to develop an optimized treatment approach to improve both mechanical performance and moisture resistance in Agave vilmoriniana fiber-reinforced composites[3].
were maintained at around 4.5 through hydrolysis induced by acetic acid. The pre-treated AVLFs were subsequently immersed in the silane solution and continuously agitated for 3 hours to facilitate bonding between silane reagent and hydroxyl groups on the fiber surface. AVLFs were cleansed with ethyl alcohol to eliminate residual silane and subsequently dried at ambient temperature for 48-50 hours. This alteration was designed to generate covalent bonds at the fiber-matrix interface[23-26].
2.4 Cassava starch coating of AVLFs
2. Materials and Methods
A surface coating composed of cassava starch was applied to AVLF’s after surface treatment to increase their hydrolytic stability and interfacial integrity. A 10% w/v cassava starch solution was prepared by dispersing the starch powder in distilled water and heating the mixture to 80 °C with continuous stirring until complete gelatinization was achieved. The silane-treated fibers were then encased in the heated starch mixture for 30 mins to ensure uniform surface coverage. After taking the fibers from the solution, the excess starch was allowed to drain and the coated AVLF’s were oven dried at room temperature for 48Hrs. The starch film was intended to serve as a biodegradable interfacial modifier which was functioning as a hydrophilic–hydrophobic transition layer to reduce water absorption and improve fiber–matrix compatibility in composite manufacturing.
2.1 Materials used
2.5 Characterization
AVLF’s were manually extracted from Agave vilmoriniana plant leaves which were locally cultivated around chettipalayam, Coimbatore, Tamil Nadu, India. Sodium Hydroxide (NaOH) and Aminopropyltriethoxysilane (APTES) were purchased from Sigma-Aldrich Chemicals Private Limited, Bengaluru, Karnataka, India for surface modification and enhancement of AVLF’s. For surface coating, Cassava Starch powder purchased from a local supplier for the AVLF’s surface coating.
2.2 Alkali treatment of AVLFs An alkali treatment with a 6% weight by volume of NaOH solution was used to improve the adhesion tendency and interfacial compatibility in Agave vilmoriniana fibres. AVLFs were immersed in the alkali at ambient temperature for 4 Hrs[11,20]. This method eliminates surface-confined polysaccharides such as hemicellulose, waxes and residual lignin that makes a rougher fibre surface and more accessible OH groups for future modification[21,22]. Subsequently, the AVLFs were thoroughly cleansed with distilled water until achieving a neutral pH which were indicating the complete removal of residual alkali. After that the AVLFs were airdried for 48 hours at ambient temperature and stored in sealed moisture-free containers.
2.3 Silane treatment of AVLFs Silane treatment was followed by NaOH treatment to improve interfacial binding and enhance the chemical interaction of AVLFs with polymer matrices. A 2% (v/v) APTES formulation was prepared using a solvent mixture of 95% ethyl alcohol and 5% water. The pH of the solution 2/9
2.5.1 Physical characteristics The fiber is long, circular, usually tapered to a tip, and has a thicker side on one side. Particularly finer fibers come from the leaf’s bottom side. Depending on the method of processing and the amount of time spent extracting the fiber, the colour of the AVLF can range from off-white to yellowish. Due to bacterial action, the treated fiber was darkened, which might be dyed with a naturally seeming light brown tint. The fiber seems robust and long-lasting. All leaf fibers have the stiff, harsh, gritty, and hard-surfaced characteristics of the dry AVLF. However, fibers become pliable, smooth, and slippery when they are wet. The diameter of the AVLF was calculated using a ZEISS (Sigma 360VP, Germany) Microscope. To take their difference in thickness into account along with single units, the dia was estimated for about 10–12 sections at 4-6 different sites of a single AVLF. The density of the AVLFs was evaluated using the conventional pycnometer methods for density measurement. Before being used, the AVLFs model was broken into pieces of 5–6 mm in length and dried out for five days in desiccators made of silica gel. In order to close the microscopic holes in the outer region, the AVLFs were then wrapped up in a container containing toluene for two hours. 2.5.2 Chemical behaviour Chemical composition analysis is essential to assess the eradication of non-cellulosic components during fiber treatments and predict performance in composite materials. The Conrad technique was used to determine the wax content of Agave vilmoriniana leaf fiber, whereas the Kurschner– Hoffner method was used to quantify the cellulose content. Polímeros, 36(2), e20260020, 2026
Surface-modified Agave vilmoriniana fibers for enhanced thermo-mechanical and interfacial performance in composites The NFT 12-008 test and the Klason method were used to measure hemicellulose and lignin. Moisture content was measured with a Sartorius MA45 analyser and ash content was measured according to ASTM E175501. 2.5.3 X-ray diffraction analysis The crystallinity and structural alterations in raw AVLFs as well as in AVLFs following surface modification by alkali, silane and starch coating were investigated by XRD. The Analysis were conducted using a diffractometer (Malvern Panalytical, Empyrean Series III, Netherlands) fitted with Bragg Brentano HD optics and a quick response detector. It provides high resolution diffraction data which facilitates a thorough comparison of the crystalline structure among various surface-modified fibres. The instrument used Cu Kα radiation with the wavelength of 1.5406 angstroms then it was powered by 45 kV and 40 mA. Diffraction traces were gathered throughout a 2θ range of 5° to 60°, enabling a thorough characterization of both crystalline and amorphous regions within the fiber structure. The degree of crystallinity was derived using the Segal empirical method. The crystallinity index is given by,
= CI ( % )
I 002 − I am ×100 I 002
(1)
where I002 is intensity of (002) crystalline peak, typically observed near 2θ ≈ 22°–23°, Iam is minimum intensity between (002) peak and amorphous background, usually near 2θ ≈ 18°. 2.5.4 Fourier transform infrared spectroscopy The chemical structure of AVLFs were examined through FTIR both before and after surface modification through alkali and silane treatment then the starch coating. The spectra was acquired using a FTIR spectrophotometer (SHIMADZU IRSpirit, Japan) attached with a single reflectance ATR measurements were performed using a QATR S accessory equipped with a diamond crystal. Each measurement was made across the spectra were recorded over the range of 4000–400 cm−1 with a precision of 4 cm−1. Each sample was averaged over 45 scans to improve signal clarity and reduce noise. The ATR sample region had a diameter of about 1.5 millimetres, which allowed for constant contact between the fibre surface and the ATR crystal. Before proceeding with the analysis, all recorded spectra were baseline adjusted with the built-in program. 2.5.5 Thermogravimetry (TG) A Thermal Analyser (NETZSCH STA 449 F3 Jupiter, Germany) were used to look at Agave vilmoriniana fibres when it exposed thermally both before and after surface modification of AVLFs through alkali and silane treatment then the starch coating. For each thermal study, a fibre sample weighing around 8 to 10 mg was put in an alumina crucible and heated from 26°C to 500°C at a steady rate of 10°C per minute under inert nitrogen environment. This technique made it possible to record changes in weight and heat flow patterns at the same time using Thermogravimetry. 2.5.6 Mechanical behaviour The tensile behaviour of single fibres were measured by universal testing equipment and adhering to ASTM D3379, Polímeros, 36(2), e20260020, 2026
the tensile behaviour of raw and surface modified AVLFs were examined. A polarised light microscope was used to measure the fibre diameters which helps to the accurate stress calculations. The experiments were examined under the temperature of 25°C and relative humidity at 65°C. At least 15 fibers from both untreated and treated AVLFs were examined to make sure the results were statistically valid. 2.5.7 Surface morphology A ZEISS (Sigma 360VP, Germany) SEM were used to examine the surface microstructure of the raw fibers as well as in AVLFs following surface modification by alkali, silane and starch coating. To improve conductivity and image clarity, raw AVLFs were spray-coated with an incredibly thin layer of gold before imaging. A secondary electron detector was used to record minute surface details during high vacuum inspections carried out at an accelerating voltage of 10 kilovolts. Each treatment produced distinct variations in surface texture, as observed in micrographs recorded at different magnifications. These observations provide visual confirmation of structural modifications and offer insight into potential enhancement of fiber–matrix adhesion in composite systems.
3. Results and Discussions 3.1 Physical characteristics In terms of effective length, the bundles of AVLFs are longer than those of Agave sisalana fibres. The AVLFs are made up of as bundles of multiple sole fibres that are tightly bound together by some waxy and sticky substances. When the fibre is physically extracted from the whole length of the leaf sheaths, the fibres from the central sheaths may vary in length from 0.5 to 1.4 meters. Using a SEM, the fibers thickness were found between 85 and 170 μm as in Figure 1. The density value of AVLFs were determined using the density bottle method at constant temperature which is not above 25° C. It shows values that on an average of 1.32 g/cc.
3.2 Chemical composition After treatment, the chemical composition of AVLFs transformed a lot. The cellulose content raised notably from 56% in untreated fibres to over 68% in fibres treated with silane and starch, while hemicellulose, lignin, and surface impurities such as waxes and ash were reduced. NaOH treatment successfully eliminated hemi-cellulose and lignin that were increasing fibre crystallinity and density to enhance fiber interlocking behaviour in composites. Silane treatment not only cleaned the AVLF surface but also enhanced fiber–matrix adhesion by introducing siloxane bonds which leads to reduce moisture uptake. Starch coating increased surface hydroxyl groups and fiber density but retained higher wax content that potentially increasing water absorption. These compositional alterations are anticipated to enhance interfacial adhesion and mechanical performance in composites, however moisture behaviour may differ. Silane-treated fibres exhibited the most efficient proportion of adhesion and hydrophobicity. A comprehensive analysis of the chemical composition among treatments is shown in the accompanying Table 1. 3/9
Saravanan, G., & Thirumalaisamy, R. 3.3 X-ray diffraction analysis The XRD analysis patterns of the untreated and treated AVLF reveal the characteristic cellulose I structure, with a prominent (002) reflection at 2θ ≈ 22–23° and a broad amorphous region around 18–19°. Untreated fibers carry more amorphous hemicellulose and lignin because it has lower (002) peak intensity. NaOH treatment raises the (002) peak and decreases the amorphous background, removing non-cellulosic components and aligning cellulose microfibrils. Crystallinity rises from 55% to 63%. Additional silane treatment increases crystallinity by 64%, revealing the cellulose structure is stable without affecting its core
crystalline phase. Fibers reach peak crystallinity (~66%) when coated with cassava starch after NaOH and silane treatment. This indicates that starch deposition does not damage the cellulose lattice and may even help order the surface fibers. The modest rise noted in silane-treated fibers is due to partial recrystallization that happens when starch retrogrades. The crystalline structure of cellulose I stays unaltered. These observations suggest that additional treatments enhance cellulose organization, aligning with the noted thermal stability and mechanical performance. The comparative XRD profiles of untreated and treated AVLFs are presented in Figure 2 for detailed analysis.
Table 1. Chemical composition of untreated, treated and starch coated AVLF’s in wt. %. Fiber Sample Untreated Alkali Treated Silane Treated Starch Coated
Cellulose 56.26 ± 1.3 67.10 ± 0.8 68.25 ± 0.6 68.32 ± 0.7
Hemicellulose 18.32 ± 1.1 10.20 ± 0.7 9.95 ± 0.5 9.82 ± 0.6
Lignin 11.02 ± 0.9 9.05 ± 0.6 7.75 ± 0.4 7.16 ± 0.5
Ash & SiO2 3.12 ± 0.5 2.45 ± 0.3 2.64 ± 0.2 2.76 ± 0.2
Wax & Others 3.87 ± 0.4 2.18 ± 0.3 1.85 ± 0.2 2.25 ± 0.3
Moisture 8.56 ± 0.6 5.25 ± 0.4 4.23 ± 0.3 5.10 ± 0.4
Figure 1. a), b), c) Different AVL Fiber’s thickness.
Figure 2. Comparison of XRD of untreated, treated and starch coated AVLF’s. 4/9
Polímeros, 36(2), e20260020, 2026
Surface-modified Agave vilmoriniana fibers for enhanced thermo-mechanical and interfacial performance in composites 3.4 Fourier transform infrared spectroscopy The FTIR spectra of AVLFs before and after surface modification and coating show clear changes in crystalline structure. The treated fibers have a stronger broad absorption band around 3300 cm−1 that corresponds to O–H stretching. This means that the cellulose hydroxyl groups are more exposed in the treated fibers. The band near 2920 cm−1 that is linked to C–H stretching is in all of the samples. In untreated fibers, a clear peak at 1730 cm−1 shows hemicellulose and waxy ester parts. The evidence that this peak gets limited after alkali and silane treatments shows that non-cellulosic parts have been removed. The absorption bands at 1610, 1235, and 1020 cm−1 are due to the stretching vibrations of lignin and the C–O bonds in cellulose and hemicellulose. An additional sharp peak around 750 cm−1 appears in silane and starch treated fibers, suggesting the formation of new chemical linkages such as Si–O bonds or starch related functional groups. These spectral changes confirm effective surface modification and indicate enhanced fiber purity and functionalization. A comparative representation of the FTIR spectra is shown in Figure 3.
3.5 Thermogravimetry This analysis of the untreated and treated Agave vilmoriniana fibers shows notable improvements in thermal stability after chemical modifications. The thermal degradation behavior of untreated and chemically treated AVLF was analyzed using TG and derivative TG (DTG). The onset degradation temperature (Tonset) was determined as an extrapolated value from TG curves using tangent intersection method at the main decomposition region. Accordingly, the Tonset of untreated fiber is around 285 °C, the NaOH treated fiber and the NaOH with silane treated fibers showed a Tonset of about 295 and 300 °C, while treated fiber with starch coated fibers exhibited a Tonset of around 300 °C.
The increase in Tonset for treated fibers suggests improved thermal stability and reduced moisture-related mass loss, indirectly indicating enhanced fiber surface modification. On otherhand, the maximum degradation temperature (Tmax) was directly obtained from the peak positions of the DTG curves, corresponding to the highest rate of mass loss. The DTG result shows Tmax values of approximately 340 °C for untreated fibers, 350 °C for NaOH treated-fibers and NaOH with silane treated fibers, 355 °C for treated and starch coated fibers. This changes confirms that the chemically treated and coated fibers were enhanced thermal stability resulting from the removal of amorphous components and improved interfacial structure, consistent with enhanced fiber–matrix bonding rather than direct hydrophobicity assessment. A comparative analysis of thermal behaviour is clearly depicted in Figure 4.
3.6 Mechanical behaviour The diameters and tensile properties such as tensile strength, Young’s modulus, and the elongation at break in raw fibers and of AVLFs following surface modification by alkali, silane and starch coating are summarized in Table 2. That the result shows a clear reduction in fiber diameter after chemical treatment, with six percent sodium hydroxide proving to be the most effective concentration among those tested. The observed reduction in fiber diameter confirms the effective removal of non cellulosic constituents such as hemicellulose and surface impurities. For mechanical characterization, five specimens from each group were tested to ensure reliable averaging of the measured properties. The treated samples have higher tensile strength and greater elongation at break than the untreated fibers. The removal of amorphous phases has made the fibers more compact and better aligned on the level of molecular structure, which has led to these improvements. This kind of structural refinement makes it easier for loads to transfer and improves the tensile mechanical performance.
Figure 3. Comparison of FTIR analysis of untreated, treated and starch coated AVLF’s. Polímeros, 36(2), e20260020, 2026
5/9
Saravanan, G., & Thirumalaisamy, R.
Figure 4. Comparison of TG and DTG of untreated, treated and starch coated AVLF’s.
Table 2. Comparison of the tensile properties of untreated, treated and starch coated AVLF’s. Fiber Sample Untreated Alkali Treated Silane Treated Starch Coated
Diameter (µm) 161 ± 16 158 ± 12 160 ± 10 162 ± 11
Tensile Strength (MPa) 358 ± 24 456 ± 22 468 ± 20 471 ± 21
3.7 Scanning Electron Microscopy analysis The SEM analysis of Agave vilmoriniana fibers shows that changes to the surface cause distinct modifications in the fiber. In the untreated fiber (Figure 5a), a thick layer of waxes, ash, and non-cellulosic materials masks the microfibrillar structure. This shows that the poor surface roughness and limited interfacial bonding potential in composites. After the alkali treatment (Figure 5b), some wax and other impurities are still there, but the surface is cleaner. This treatment breaks up the amorphous hemicellulose matrix, making the fibrillar cellulose more visible. Silane-treated fibers (Figure 5c) have surfaces that are much rougher and have visible cellulose microfibrils. This is because the silane coupling agent interacts with hydroxyl groups, which creates covalent bonding sites that help the matrix bind better. Starch-coated fibers (Figure 5d) have smoother, more continuous surfaces with fewer voids and microfibrils that are well-aligned. This means that the coating looks uniform and there are fewer surface defects which were drastic changes while comparing with the raw fiber (Figure 5a). The starch film probably makes things more compatible by forming hydrogen bonds with polar matrices.
4. Conclusions The comprehensive study of Agave vilmoriniana fibers shows that certain chemical modifications have a significant 6/9
Young’s Modulus (GPa) 18.12 ± 1.1 20.23 ± 0.9 21.56 ± 0.8 23.42 ± 0.9
Elongation at Break (%) 3.17 ± 0.4 3.81 ± 0.3 3.85 ± 0.2 4.12 ± 0.3
positive effect on their structural, thermal and mechanical characteristics, based on their applicability as eco-friendly reinforcing agents in polymer composites. The alkali treatment enhances cellulose, crystallinity, tensile strength, modulus, and thermal stability by removing the non-cellulosic materials, such as hemicellulose and lignin. Silane treatment is used to promote the development of covalent siloxane bonding, promote bonding of the fibers and the matrix have increase the composite durability and reduce the moisture affinity. The coating of starch increases the coverage and interfacial compatibility. Presumably, because of the limited starch retrogradation their effect on the total thermal and structural properties is not significant in the current conditions of processing. FTIR Spectroscopy and XRD postulates that the surface treatments lead to changes in the chemical and crystalline structure. The thermogravimetry has shown that the treated fibers are more stable at higher temperatures with the alkali treatment showing significant enhancement. SEM explains that the process gradually removes the surface contaminants and improve the surface roughness. This makes the composite matrix mechanically interlock with the surface. The physicochemical properties of Agave vilmoriniana fibers are increased by the treatment induced changes, which confirms its feasibility as a sustainable reinforcement material. It has been found that surface-engineered plant-based fibers can be effectively used as reinforcements in bio-composites that would require improved mechanical performance, durability, and thermal stability where used in engineering. Polímeros, 36(2), e20260020, 2026
Surface-modified Agave vilmoriniana fibers for enhanced thermo-mechanical and interfacial performance in composites
Figure 5. SEM image of a) untreated AVLF, b) NaOH treated AVLF, c) Silane treated AVLF and d) starch coated AVLF. Polímeros, 36(2), e20260020, 2026
7/9
Saravanan, G., & Thirumalaisamy, R.
5. Author’s Contribution • Conceptualization – Gowtham Saravanan • Data curation – Gowtham Saravanan • Formal analysis – Gowtham Saravanan • Funding acquisition – NA • Investigation – Gowtham Saravanan • Methodology – Gowtham Saravanan; Ramakrishnan Thirumalaisamy • Project administration – Gowtham Saravanan • Resources – Gowtham Saravanan; Ramakrishnan Thirumalaisamy • Software – Gowtham Saravanan • Supervision – Ramakrishnan Thirumalaisamy • Validation – Ramakrishnan Thirumalaisamy • Visualization – Gowtham Saravanan; Ramakrishnan Thirumalaisamy • Writing – original draft – Gowtham Saravanan • Writing – review & editing – Gowtham Saravanan; Ramakrishnan Thirumalaisamy
7. References 1. Kumar, P., Gupta, H. S., Singh, M., Chaudhari, A. S., Maurya, A. K., & Manik, G. (2024). Mechanical, thermal, and morphological analysis of Himalayan Agave fiber/GO coated fly ash hybrid polypropylene composites. Chemistry (Weinheim an der Bergstrasse, Germany), 31(2), e202402393. http://doi.org/10.1002/chem.202402393. PMid:39489704. 2. Ramakrishnan, T., & Aravinth, K. (2023). Study on properties of new biodegradable plant fiber (Agave decipiens) for polymer reinforcement. Global NEST Journal, 25(9), 31-40. http://doi. org/10.30955/gnj.005219. 3. Ramesh, M., Tamil Selvan, M., & Niranjana, K. (2022). Thermal characterization and hygrothermal aging of lignocellulosic Agave Cantala fiber reinforced polylactide composites. Polymer Composites, 43(9), 6453-6463. http://doi.org/10.1002/pc.26958. 4. Prasad, L., Singh, V., Patel, R. V., Yadav, A., Kumar, V., & Winczek, J. (2023). Physical and mechanical properties of rambans (agave) fiber reinforced with polyester composite materials. Journal of Natural Fibers, 19(13), 6104-6118. http://doi.org/10.1080/15440478.2021.1904481. 5. Ravi, P., Arumugam, E., & Katiyar, J. K. (2024). Investigation of physical, mechanical, tribological and biodegradable properties of hybrid natural fibre reinforced polymer composite. Tribology - Materials, Surfaces & Interfaces, 18(2), 79-92. http://doi.org/10.1177/17515831241241945. 6. Yadav, J., Ramkumar, P. L., & Parwani, A. K. (2024). Characterization of Azadirachta indica natural cellulosic fiber and its polymer composites. Arabian Journal for Science and Engineering, 50(17), 13635-13647. http://doi.org/10.1007/s13369-024-09487-4. 7. Rangappa, S. M., Siengchin, S., Parameswaranpillai, J., Jawaid, M., & Ozbakkaloglu, T. (2022). Lignocellulosic fiber reinforced composites: Progress, performance, properties, applications, and future perspectives. Polymer Composites, 43(2), 645-691. http://doi.org/10.1002/pc.26413. 8. Gowtham, S., Jeevanantham, T., Emelda, J., & Edric, J. (2024). Investigation on effect of fibre orientation on mechanical behaviour of polymer matrix natural fibre reinforced composite material. Materials Today: Proceedings. Advance online publication. http://doi.org/10.1016/j.matpr.2024.04.022. 8/9
9. Ramakrishnan, T., Babu, M. S., Balasubramani, S., Manickaraj, K., & Jeyakumar, R. (2021). Effect of fiber orientation and mechanical properties of natural fiber reinforced polymer composites: a review. Paideumajournal, 14(3), 17-23. Retrieved in 2025, December 4, from https://paideumajournal.com/ gallery/3-mar2021.pdf 10. Ali, A., Shaker, K., Nawab, Y., Jabbar, M., Hussain, T., Militky, J., & Baheti, V. (2018). Hydrophobic treatment of natural fibers and their composites: a review. Journal of Industrial Textiles, 47(8), 2153-2183. http://doi.org/10.1177/1528083716654468. 11. Ramakrishnan, T., & Sampath, P. S. (2017). Dry sliding wear characteristics of new short agave angustifolia marginata (AAM) fiber-reinforced polymer matrix composite material. Journal of Biobased Materials and Bioenergy, 11(5), 391-399. http://doi.org/10.1166/jbmb.2017.1699. 12. Sanjay, M. R., Madhu, P., Jawaid, M., Senthamaraikannan, P., Senthil, S., & Pradeep, S. (2018). Characterization and properties of natural fiber polymer composites: a comprehensive review. Journal of Cleaner Production, 172, 566-581. http:// doi.org/10.1016/j.jclepro.2017.10.101. 13. Lee, C. H., Khalina, A., & Lee, S. H. (2021). Importance of interfacial adhesion condition on characterization of plant-fiber-reinforced polymer composites: a review. Polymers, 13(3), 438. http://doi.org/10.3390/polym13030438. PMid:33573036. 14. Hosseini, S. B., Gaff, M., Li, H., & Hui, D. (2023). Effect of fiber treatment on physical and mechanical properties of natural fiber-reinforced composites: a review. Reviews on Advanced Materials Science, 62(1), 20230131. http://doi.org/10.1515/ rams-2023-0131. 15. Kamarudin, S. H., Mohd Basri, M. S. M., Rayung, M., Abu, F., Ahmad, S., Norizan, M. N., Osman, S., Sarifuddin, N., Mat Desa, M. S. Z., Abdullah, U. H., Tawakkal, I. S. M. A., & Abdullah, L. C. (2022). A review on natural fiber reinforced polymer composites (NFRPC) for sustainable industrial applications. Polymers, 14(17), 3698. http://doi.org/10.3390/ polym14173698. PMid:36080773. 16. Kabir, M. M., Wang, H., Lau, K. T., & Cardona, F. (2012). Chemical treatments on plant-based natural fibre reinforced polymer composites: an overview. Composites. Part B, Engineering, 43(7), 2883-2892. http://doi.org/10.1016/j. compositesb.2012.04.053. 17. Thirumalaisamy, R., Kumar, S. S., Chelladurai, S. J. S., Gnanasekaran, S., Sivananthan, S., Geetha, N. K., Ramesh, A., & Assefa, G. B. (2023). Study on water absorption characteristics, various chemical treatments, and applications of biological fiber‐reinforced polymer matrix composites. Journal of Nanomaterials, 2023, 9903119. http://doi. org/10.1155/2023/9903119. 18. Prabu, R., Yuvaraj, G., Saravanan, G., & Pradhan, R. (2025). Influence of silane functionalized heat treated biosilica on mechanical, wear, and dynamic load–bearing properties of nettle fibre–reinforced vinyl ester composites. Biomass Conversion and Biorefinery, 15(3), 4867-4880. http://doi. org/10.1007/s13399-024-06243-4. 19. Gowtham, S., Kumar, T. Ch. A., Devi, N. S. M. P. L., Chakravarthi, M. K., Pradeep Kumar, S., Karthik, R., Anandaram, H., Kumar, N. M., & Ramaswamy, K. (2022). A survey on additively manufactured nanocomposite biomaterial for orthopaedic applications. Journal of Nanomaterials, 2022(1), 8998451. http://doi.org/10.1155/2022/8998451. 20. Jani, S. P., Sujin, J. A., Rajaganapathy, C., & Khan, A. M. (2024). Development of hybrid composite with natural fillers for mechanical property and machinability study. Progress in Rubber, Plastics and Recycling Technology, 40(1), 17-32. http://doi.org/10.1177/14777606231186633. Polímeros, 36(2), e20260020, 2026
Surface-modified Agave vilmoriniana fibers for enhanced thermo-mechanical and interfacial performance in composites 21. Madhu, P., Sanjay, M. R., Jawaid, M., Siengchin, S., Khan, A., & Pruncu, C. I. (2020). A new study on effect of various chemical treatments on Agave Americana fiber for composite reinforcement: physico-chemical, thermal, mechanical and morphological properties. Polymer Testing, 85, 106437. http://doi.org/10.1016/j.polymertesting.2020.106437. 22. Saravanan, G., Thirumalaisamy, R., Devaraj, T. V., Shanmugam, C., Subramaniyan, R., Kalimuthu, K. R., & Pathan, N. S. (2024). Investigation on morphological and tensile properties of chemically treated Borassus Flabellifer Lontar fruit fibers. Matéria, 29(3), e20240166. http://doi.org/10.1590/1517-7076rmat-2024-0166. 23. Nurazzi, N. M., Shazleen, S. S., Aisyah, H. A., Asyraf, M. R. M., Sabaruddin, F. A., Mohidem, N. A., Norrrahim, M. N. F., Kamarudin, S. H., Ilyas, R. A., Ishak, M. R., Abdullah, N., & Nor, N. M. (2021). Effect of silane treatments on mechanical performance of kenaf fibre reinforced polymer composites: a review. Functional Composites and Structures, 3(4), 045003. http://doi.org/10.1088/2631-6331/ac351b. 24. Latif, R., Wakeel, S., Zaman Khan, N., Noor Siddiquee, A., Lal Verma, S., & Akhtar Khan, Z. (2019). Surface
Polímeros, 36(2), e20260020, 2026
treatments of plant fibers and their effects on mechanical properties of fiber-reinforced composites: A review. Journal of Reinforced Plastics and Composites, 38(1), 15-30. http://doi.org/10.1177/0731684418802022. 25. Yadav, S. N., Arya, S., Chawla, V. K., & Kushwaha, P. K. (2024). Characterization of injection moulded bamboo and tire rubber reinforced plastic composites. Journal of the Indian Academy of Wood Science, 21(1), 224-233. http://doi. org/10.1007/s13196-024-00342-5. 26. Sanjay, M. R., Siengchin, S., Parameswaranpillai, J., Jawaid, M., Pruncu, C. I., & Khan, A. (2019). A comprehensive review of techniques for natural fibers as reinforcement in composites: preparation, processing and characterization. Carbohydrate Polymers, 207, 108-121. http://doi.org/10.1016/j. carbpol.2018.11.083. PMid:30599990. Received: Dec. 04, 2025 Revised: Feb. 07, 2026 Accepted: Feb. 19, 2026 Editor-in-Chief: Sebastião V. Canevarolo
9/9
ISSN 1678-5169 (Online)
https://doi.org/10.1590/0104-1428.20250061
Innovations in sustainable additive manufacturing: PLA, Amazon wood waste, Brazil nut oil Jackeline Lira Bremgartner1,2,3 , Joaquim dos Santos1,2 , Lizandro Manzato3 Vitor Bremgartner3 and Claudete Catanhede do Nascimento2 Programa de Pós-graduação em Ciências de Florestas Tropicais - CFT, Instituto Nacional de Pesquisas da Amazônia - INPA, Manaus, AM, Brasil 2 Instituto Nacional de Pesquisas da Amazônia - INPA, Manaus, AM, Brasil 3 Laboratório de Síntese e Caracterização de Nanomateriais - LSCN, Polo de Inovação, Instituto Federal de Educação, Ciência e Tecnologia do Amazonas - IFAM, Manaus, AM, Brasil *jackelinelirabref@gmail.com
1
Abstract Responding to the growing interest in lignocellulosic materials for 3D printing, this research addresses the need for sustainable solutions, employing Amazonian wood waste and Brazil nut oil (BNO) as a natural binder for polylactic acid (PLA). We successfully developed filaments from a composition of 4% powdered sawdust of Nectandra rubra and Zygia racemosa, respectively with medium and high density, with 91% PLA and 5% BNO, which were extruded and printed. Physical-mechanical and characterization tests were performed using SEM, TGA, and FTIR. The incorporation of wood increased flexural strength, but reduced compression and tensile strength. FTIR analysis showed compatibility between the components, although the addition of wood caused agglomeration as indicated by SEM. The high-density species increased the thermal stability, as indicated by TGA. This study confirms the potential of filament developed with Amazonian woods and BNO, opening new avenues for sustainable additive manufacturing. Keywords: 3D printing, biocomposite, extrusion, polymers, vegetable oil. Data Availability: All data supporting the findings of this study are available from the corresponding author upon request How to cite: Bremgartner, J. L., Santos, J., Manzato, L., Bremgartner, V., & Nascimento, C. C. (2026). Innovations in sustainable additive manufacturing: PLA, Amazon wood waste, Brazil nut oil. Polímeros: Ciência e Tecnologia, 36(2), e20260021. https://doi.org/10.1590/0104-1428.20250061
1. Introduction Among the various 3D printing techniques, also known as Additive Manufacturing (AM), Fused Deposition Modeling (FDM) stands out. FDM involves the extrusion of a thermoplastic filament, which is melted and precisely deposited, layer by layer, onto a platform[1,2]. This technique has several applications in sectors such as automotive, aeronautical, construction, culinary arts, clothing, and medical engineering[3-6]. PLA (polylactic acid) biopolymer is one of the most widely used in FDM, derived from corn starch or sugarcane, and stands out for its biodegradability, non-toxicity, and biocompatibility. It is processed industrially by extrusion or injection molding. The mechanical and thermal properties, ease of molding, and print quality of PLA are some of the characteristics that make it attractive for use compared to petroleum-derived plastics[1,7]. PLA mixed with wood powder and synthetic or natural binders has the potential to form composites and transform them into filaments using extruders[3]. Studies show the use of PLA as a matrix in combination with wood as reinforcement[7-10] in the manufacture of filaments for 3D printing. Despite these advances, there is a notable gap in
Polímeros, 36(2), e20260021, 2026
the application of this technique with Amazonian tropical woods from forest management areas. In sawmills in the Brazilian Amazon, wood waste can represent about 60 to 70% of industrialized logs processing[11-13]. Furthermore, there are few studies on the use of wood waste in AM, however, the reuse of wood waste in polymeric matrices is promising for AM[2]. Some works indicate applications in 3D printing of wood species in combination with polymers, adhesives, plaster, cellulose, cement, lignin, sodium silicate, maleic anhydride, epoxy resin, polyurethane, vinyl acetate, among others[3]. Therefore, it is noted that mostly non-biodegradable and even toxic substances are used to manufacture filaments, as well as the absence of vegetable oil binder in additive manufacturing. For the manufacture of a biocomposite, the addition of a binding agent is necessary to improve the adhesion between the wood incorporated into the PLA[9,10]. In turn, natural Brazil nut oil, Bertholletia excelsa, (BNO) has the potential to act as a binding agent between sawdust and PLA, promoting a more homogeneous filament, since it was used for the first time as a natural binder in 3D printing
1/10
O O O O O O O O O O O O O O O O
Bremgartner, J. L., Santos, J., Manzato, L., Bremgartner, V., & Nascimento, C. C. in this research.. BNO is a regional raw material from the Amazon, biodegradable, non-toxic and has antioxidant, plasticizing and lubricating properties[14]. In addition, this oil is applied as a biofuel and in the food, cosmetic and pharmaceutical industries[14-16]. Studies show satisfactory technological characteristics of wood/PLA in AM. Ramaux et al.[2] show that the wood species and particle size affect the properties of the printing composite. Narlıoğlu et al.[17] concluded that the addition of Pinus nigra (medium density) sawdust in a proportion of 0–20% to PLA, made in a twin-screw extruder, reduced tensile strength and increased flexural strength, acting as an adequate and sustainable reinforcement for high-quality 3D filaments. Tao et al.[10] extruded PLA and 5% of 14 µm Aspen wood sawdust (low density) in a PLA matrix using a single-screw extruder and identified that the addition of wood increased flexural strength but reduced tensile strength, with a decrease in thermal stability with the addition of wood. Some works[18,19] with commercial filament of 40% wood fiber and 60% PLA showed that printing speed affects appearance, density and compression strength, while tensile and flexural strength are little influenced; however, these properties decrease with increasing extrusion temperature due to thermal degradation of the fibers.
So, this research aims to investigate the feasibility of composite manufacturing from powdered wood waste of Amazonian species, in combination with virgin PLA pellets, and the addition of BNO, in order to develop a sustainable filament for application in 3D printing.
2. Materials and Methods 2.1 Materials The wood waste used in this study was sourced from Precious Woods (Mil Madeiras), a forest management company located in Itacoatiara, Amazonas, Brazil, and certified by the Forest Stewardship Council (FSC). Initially, the length, width, and thickness of the sawmill’s mechanical processing waste were measured using a tape measure to quantify its volume (Figure 1a). Subsequently, in the band saw machinery (Figure 1b), test specimens were cut from the collected waste in an oriented manner in the planes (transverse, tangential and radial) in dimensions of 2 cm x 2 cm x 2 cm (Figure 1c). The samples were sent for wood identification, confirming the species Zygia racemosa (Angelim rajado), family Fabaceae, density of 0.95 to 1.00 g/cm3 (high) and the species Nectranda rubra (Louro gamela), family Lauraceae, density of 0.65 g/cm3 (medium).
Figure 1. Steps taken from obtaining the residues to the granulometry of the species. 2/10
Polímeros, 36(2), e20260021, 2026
Innovations in sustainable additive manufacturing: PLA, Amazon wood waste, Brazil nut oil The volume of wood residues was approximately 7050 cm3 and 10816 cm3 for Z. racemosa and N. rubra, respectively. Subsequently, the wood waste was processed into shavings using planer-trowel equipment (Figure 1d) to facilitate grinding in an ACB Labor brand rotary knife mill, yielding sawdust (Figure 1e). The sawdust of each species was sieved through 150 μm openings, obtaining the sawdust powder (Figure 1f). The PLA pellets in natural color are from the North American company NatureWorks, imported by the Brazilian company 3D LAB. PLA has a melting temperature of 165°C - 180°C, glass transition (Tg) of 55°C - 65°C and density of 1.24 g/cm3. Each distinct formulation (in %wt) was assigned a specific nomenclature, being: 1 (PLA 100%); formulation 1: N.rubra (4% sawdust, 91% PLA and 5% BNO); formulation 2: Z.racemosa (4% sawdust, 91% PLA and 5% BNO).
2.2 Methods 2.2.1 Extrusion Before each extrusion, the PLA pellets were dried at 90 °C for 2 hours and sawdust were dried at 103 °C for 24 hours (Figure 2). The BNO with 5% was manually mixed with 91% of pellets and 4% of sawdust powder (150 µm). These formulated proportions proved to have no impact on 3D printing, as they did not clog the 3D printer. The formulation was fed into the extruder, where the mixture was detailed by the single-screw extruder and melted in the heater, exiting through the nozzle as a ±1.75 mm filament, which received a thermal shock from the fan and was manually wound. During the extrusions, adjustments to the screw speed and extruder temperature were necessary when the filament became too soft or had incompletely fused parts, causing losses. The extrusion temperatures of the PLA pellets ranged between 285 °C and 290 °C. The species Z. racemosa presented greater manufacturing difficulty during extrusion, as the filaments broke more frequently compared to N. rubra, ranging from 300 °C to 295 °C for Z. racemosa and from 295 °C to 290 °C for N. rubra. The high temperature required can be explained by the equipment not being robust at the industrial level, as well as the composition of species may have been affected,
with the species (Z. racemosa) having thick fibers, more closed ducts and high density[20] requiring a higher extrusion temperature. On the other hand, the ease of extrusion of N. rubra can be explained by the thin to medium-walled fibers and more open pores, being an easy-to-work wood[21]. In PLA extrusion, the pellets were extruded at a temperature of 290 °C and screw rotation speeds ranging from 8.42 rpm to 25.10 rpm to adjust the filament diameter as close as possible to 1.75 mm. 2.2.2 3D printing of samples by FDM 3D objects were graphically modeled using Ultimaker Cura software in order to 3D printer could receive commands and print the objects. Filaments with a composition of 4% sawdust, 5% BNO, and 91% PLA (for both species) were printed using a Creality Ender 3 3D printer (Figure 3a), using the FDM method, following 3D printing parameters. During 3D printing (Figure 3b), the filament passes through a heating block attached to the printer at a temperature of 200ºC that melts it and is transferred to a nozzle with a diameter of 0.4 mm, at a printing speed of 50 mm/s, with a ±45º raster angle, and deposits the extruded material layer by layer of 0.2 mm (except the first layer, which is 0.4 mm) on top of a hot platform with a temperature of 60ºC that moves during printing in the x, y and z directions until forming the object with 100% filled. Figures 3c, 3d, 3e show the printed samples for the mechanical, physical and characterization tests for each formulation.
2.3 Physical properties Printed samples measuring 36 mm x 12.5 mm x 6 mm were used in all physical tests. Apparent density of these samples were obtained by measuring the mass on an analytical balance and measuring the volume (length, width and thickness) using a digital caliper and specimeter, and calculating the mass and volume ratio using Equation 1: D = M /V
(1)
where: D: density (g/cm3); M: mass (g); V: volume (cm3). Absorption and swelling were determined by ASTM 1037. Test specimens were measured in mass and volume
Figure 2. Steps to develop filament: (a) preparation of mixtures; (b) equipment used: extruder with temperature panel and feeder, external fan; (c) filaments. Polímeros, 36(2), e20260021, 2026
3/10
Bremgartner, J. L., Santos, J., Manzato, L., Bremgartner, V., & Nascimento, C. C.
Figure 3. (a) 3D printer. (b) 3D printing and (c), (d), (e) printed test specimens.
before and after immersion in distilled water for 2 hours, plus an additional period of 22 hours (total of 24 hours), with removal of excess water from the sample on filter paper. The values of thickness swelling were obtained according to Equation 2: T1 − T 0 Ts = x100 T0
(2)
where, Ts: thickness swelling of the test specimen (%); T1: thickness of the test specimen after immersion (mm); T0: thickness of the test specimen before immersion (mm). The water absorption were obtained according to Equation 3: M1− M 0 Wa = x100 M0
(3)
where, Wa: water absorption (%); M1: mass of the test specimen after immersion (g); M0: mass of the test specimen prior to immersion (g). The moisture content of the filaments and printed parts (or samples) were obtained on Shimadzu’s MOC63 moisture determination scale, with calibration at 50°C for 15 minutes, presenting the moisture value in percentage and a margin of error of 0.1%.
2.4 Mechanical properties The tensile test was followed in accordance with the ASTM D638 standard on samples with dimensions of 114.3 mm x 19.5 mm x 4.064 mm, with application of the type IV test, using a speed of 5 mm/min, a span of 50 mm and a load cell of 2 kN in the Instron machine, model 5564 and determining the tensile strength (TS) and the tensile modulus (TM). In the compression test, the ASTM D695 standard was used. Samples with dimensions of 12.7 mm x 12.7 mm x 25.4 mm were tested in the vertical direction at a speed of 1.3 mm/min and a load cell of 100 kN in the Instron machine, model EMIC 2300 and obtaining the compressive strength (CS) and the compressive modulus (CM). In the flexural test, the ASTM D790 standard was used to determine the Modulus of Rupture (MOR) and Modulus of Elasticity (MOE) with a 2 kN load cell on the Instron machine, model 5564. Test specimens with rectangular dimensions of 80 mm × 10 mm × 4 mm were tested and 4/10
supported in a 57 mm span to receive the application of a concentrated load in the middle of the sample at a speed of 1.53 mm/min.
2.5 Scanning Electron Microscopy (SEM) Test Printed samples were metallized with a thin layer of gold to enhance electron conductivity, and morphological images of their surface structures were generated using a JSM IT500 HR microscope.
2.6 Thermogravimetric Analysis (TGA) We observed the stages of thermal degradation (mass loss) of the printed samples with masses around 11 mg in the Shimadzu TGA-50 thermal analyzer, starting the process by heating at a rate of 10°C/min until reaching a temperature of 500°C.
2.7 Fourier Transform Infrared (FTIR) Spectroscopy Functional groups and chemical bonds in the printed samples and sawdust powder from both species were analyzed via Fourier Transform Infrared (FTIR) Spectroscopy using the Attenuated Total Reflectance (ATR) technique. Measurements were performed on an Agilent Technologies Cary 630 instrument in the range of 4000 to 650 cm−1 with 128 scans.
2.8 Statistical analysis We used the OriginPro 2023b and R Studio programs. We performed Analysis of Variance (ANOVA) with Tukey’s test, with p < 0.05 significant for PLA and the formulations of N.rubra and Z.racemosa with 5 repetitions of the physical test, totaling 15 samples. 5 repetitions were used for each mechanical test, totaling 45 samples. The characterization was analyzed based on the observations of the graphs generated from 1 sample of each formulation.
3. Results and Discussions 3.1 Filament diameters The diameters for PLA filaments comprised a frequency around 1.65 ± 10 mm. The species N.rubra obtained diameters between 1.55 mm and 1.70 mm. Z.racemosa obtained a frequency of diameter of 1.60 ± 10 mm. Despite the variations in diameters, it was possible to print the 3D parts. Polímeros, 36(2), e20260021, 2026
Innovations in sustainable additive manufacturing: PLA, Amazon wood waste, Brazil nut oil 3.2 Physical properties The PLA presented a density of 0.842 g/cm in Table 1, which was lower than that found in the theoretical density between 1.23 and 1.24 g/cm3[22]. The density 0.96 g/cm3 of N.rubra of the printed part was the highest among the formulations, since the sawdust powder added to the PLA contributed to this increase, being significant between formulations. The printed part of Z. racemosa presented a density of 0.845 g/cm3, which suggests that the difficulty in extruding this species and the variations in filament diameters may have consequences in not increasing density as observed for N.rubra. For comparison purposes, the commercial filament of 40% wood fibers and 60% PLA has a density of 1.20 g/cm3, changing values w ith increasing printing speed with speeds of 30, 50 and 70 mm/s and densities of 1.06, 1.02 and 1.0 g/cm3, respectively[18]. The quality and mechanical properties of FDM-printed components are influenced by density and several printing parameters[19]. Therefore, density plays an important role in material performance, as it will be influenced by voids, weight, printing defects, extrusion quality, among others. 3
The moisture content of the filaments and 3D printed parts was low and not significant. PLA had the highest moisture content of the filaments at 1.07%, followed by Z.racemosa with 0.96% and 0.72% for N.rubra (Table 1). The moisture content of the printed parts was similar between formulations, showing that moisture content decreased after 3D printing. Drying the pellets and sawdust powder
before extrusion may have contributed to a material with low moisture content, as well as storing the pellets to avoid absorbing moisture and the printed parts in airtight bags with silica. The moisture content results from printed parts are below when compared to those in the literature. According to Yang[19], moisture content of 2.1% and 1.9% was obtained for samples printed with PLA and Cedrela spp. at 200°C and 210°C, respectively, and no significant differences were observed. Wood parts printed with PLA subjected to a temperature of 20°C and relative humidity (RH) of 33%, 65% and 85% increased from 0.8 to 1.6%, 1.4 to 3% and 2 to 4%, respectively[10]. The printed parts of PLA and Z.racemosa absorbed more water and swelled in thickness compared to N.rubra. However, the results shown in Table 2 did not show significant differences in absorption and swelling of the printed samples after 2 h and 24 h, evidencing that the biocomposite parts of the Amazonian species studied can swell and shrink in thickness and absorb water in a similar way to PLA parts.
3.3 Mechanical properties The results of the tensile, compression, and flexural tests of the printed samples are shown in Table 3. In tensile testing, PLA showed higher TS and TM values among the formulations; however, PLA had a lower TS when compared to the literature, since tensile in other works strength is approximately 50 to 70 MPa[22] and 44.2 MPa[19]. It also had a lower TM when compared to the value reported in the PLA pellet manufacturer’s DataSheet, which is around 1896 MPa.
Table 1. ANOVA results of density, moisture of filaments and printed samples. Formulations
Density*(g/cm3)
Filament moisture*(%)
Moisture printed samples*(%)
PLA Nr/OCB Zr/OCB
0.842 ± 0.053 b 0.96 ± 0.058 a 0.846 ± 0.059 b
1.07 ± 0.608 a 0.72 ± 0.388 a 0.96 ± 0.288 a
0.41± 0.06 a 0.32 ± 0.108 a 0.31 ± 0.117 a
*Values are mean ± standard deviation (S) with (n = 5). Same letter in each column is not statistically different at a significance level of p < 0.05 between formulations according to the Tukey test.
Table 2. ANOVA results of each absorption and thickness swelling formulations. Formulations PLA N.rubra Z.racemosa
Water Absorption (Wa)* 2h 24 h 3.06 ± 1.16 a 5.67 ± 3.01 a 2.10 ± 0.439 a 4.87 ± 2.44 a 3.77 ± 0.14 a 7.94 ± 1.48 a
Thickness Swelling (Ts)* 2h 24 h 0.10 ± 0.164 a 0.15 ± 0.030 a 0.03 ± 0.020 a 0.09 ± 0.053 a 0.06 ± 0.062 a 0.11 ± 0.065 a
*Values are mean ± standard deviation (S) with (n = 5). Same letter in each column is not statistically different at a significance level of p < 0.05 between formulations according to the Tukey test.
Table 3. ANOVA results for each mechanical test formulations. Formulations PLA N.rubra Z.racemosa
Tensile Properties* TS (MPa) TM (MPa) 12.2 ± 1.30 a 794 ± 65 a 407 ± 320 b 7.56 ± 1.90 b 687 ± 133 ab 7.76± 1.60 b
Compression Properties* CS (MPa) CM (MPa) 28.09 ± 13.7 a 793.66 ± 312 a 17.23 ± 4.25 a 503.54 ± 145 ab 12.34 ± 8.53 a 298.26 ± 96 b
Flexural Properties* MOR (MPa) MOE (MPa) 33.97 ± 18.3 a 963.59 ± 388 b 34.4± 4.09 a 1478.28 ± 78.8 a 38.58± 6.75 a 1496.84 ± 131 a
*Values are mean ± standard deviation (S) with (n = 5). Same letter in each column are not statistically different at a significance level of p < 0.05 between formulations according to the Tukey test.
Polímeros, 36(2), e20260021, 2026
5/10
Bremgartner, J. L., Santos, J., Manzato, L., Bremgartner, V., & Nascimento, C. C. This aspect may be associated with the void in the samples and the oscillations in the diameters of the filaments that feed the samples during 3D printing with less or more material, in addition to the high temperature used in the extruder at the laboratory level causing thermal degradation. Similar behavior was observed by Agaliotis et al.[23], in which the TS was lower than the value reported by the manufacturer, which was attributed to the void in the part. Wood formulations showed lower TS and TM than PLA, which may be associated with the lack of long fibers in the wood, making them less resistant when force is applied in opposite directions. In the study by Yang and Yeh[18], the TS of the wood/PLA filament with contents of 30, 50 and 70% ranged from 19.2 MPa to 19.8 MPa and the TM from 1650 MPa to 1731 MPa. Most PLA tensile samples and species broke in the transverse direction (Figure 4). In compression, we noted that CS of the wood formulations was lower than PLA, although not significantly so. For CM, the values of the species were lower than those of PLA, however, with a significant difference between Z. racemosa and PLA. The voids caused by the variation in filament diameter as well as the low density caused delamination of the parts in the form of lines in both the wood formulations and PLA (Figure 4), as the compressive load was applied. In the literature, Agaliotis et al.[23] found mechanical reduction due to the formation of voids between the layers and the reduction in molecular weight due to extrusion and printing. Regarding flexural tests, Table 3 shows that addition of wood increased the elastic capacity of 3D parts. The MOE values of N. rubra and Z. racemosa was 153% and 155% higher than PLA, respectively, with a significant difference compared to PLA. The MOR values d id not show a significant difference, highlighting that Z. racemosa presented a
higher MOR among the formulations. The results of the formulations with wood in this research are close to the commercial wood/PLA filament found by Yang and Yeh[18] (32.3 to 34 MPa), but slightly lower in MOE (1575 to 1680 MPa). Furthermore, the samples with wood showed more prominent bending, corroborating the elastic capacity of the material (Figure 4). Agglomerations resulting from the addition of wood in the printed layers, visualized in SEM, indicate a weak interface according to Tao et al.[10], which may have affected the mechanical properties. Also, thermal degradation may have influenced the mechanical properties due to the high temperatures used in the extruder to manufacture the filaments, as well as variations in diameters that caused voids in the filler layers. Furthermore, the mechanical properties are strongly dependent on the printing orientation (0°, 45° and 90°) due to anisotropy, and in this research a ±45° angle was used. The filament manufacturing process in large industrial extruders with automated temperatures and speeds may reduce the need for adjustments during filament production and allow for the use of lower temperatures and more homogeneous filaments.
3.4 Scanning Electron Microscopy (SEM) Test We verified the morphology of the composites through the microstructure of the printed parts. In the PLA part, we identified pieces that were not completely fused, as shown in Figure 5a. In Figure 5b of N. rubra and Figure 5c of Z. racemosa, we verified agglomerations of pellet pieces with wood powder and a more uniform printing layer of N. rubra. However, it was possible to print the parts with potential for use, showing that the granulometry and amount of wood
Figure 4. Physical state of the samples after mechanical testing for each formulation (a), (b), (c). From top to bottom: tensile, compression, and flexural results. 6/10
Polímeros, 36(2), e20260021, 2026
Innovations in sustainable additive manufacturing: PLA, Amazon wood waste, Brazil nut oil
Figure 5. Microscopy of printed parts: (a) PLA; (b) N.rubra; (c) Z.racemosa.
proportion were satisfactory. Variations in fiber diameter, workability, and residual lignin content can interfere with layer continuity in 3D printing, as heated wood fibers cause thermal changes in the process[18].
3.5 Thermogravimetric analysis (TGA and DTG) In the first stage of PLA degradation, the water contained in the material was removed, while in second stage the degradation of the molecular chain occurred. After, total degradation occurred, resulting in carbonization process in ashes[10]. The thermal degradation of PLA had an initial temperature (Ti) of 295°C and mass loss (Tdeg) of 364°C, with a maximum peak of derived thermogravimetry (DTG) of 348°C, intermediate in relation to the other formulations, and presented a less loss of residue after carbonization of 95% in relation to the composites, with a final temperature (Tf) of 420°C (Figure 6a). For wood, thermal degradation typically involves distinct stages: the evaporation of water and volatile compounds between 100°C and 200°C, followed by the complete degradation of hemicellulose in the range of 200°C to 300°C[24,25]. Cellulose degradation generally commences between 300°C and 400°C[24], while lignin degradation occurs over a broader range of 300°C to 500°C[26]. With the addition of wood, N. rubra showed an initial decomposition of 278°C and mass loss at 331°C, with a final residual mass 45% higher at 446°C compared to PLA and Z. racemosa (Figure 6a). DTG curve shows that the maximum decomposition rate peaked at around 311°C (Figure 6b). Comparing with related works, Tao et al.[10] reported that sawdust from the species Populus spp., with a low to medium wood density between 0.36 and 0.56 g/cm3 in combination with PLA, showed a lower temperature and Polímeros, 36(2), e20260021, 2026
higher residual mass compared to pure PLA. The commercial PLA filament with cedar fibers Cedrela spp. had mass loss above 240°C, while the wood of this species has an average density between 0.43 g/cm3 and 0.52 g/cm3[19]. The low thermal stability and high residual mass of these species were similar to N.rubra. There was an increase in the thermal stability of the composite and lower residual loss of Z.racemosa when compared to N.rubra. In turn, Z.racemosa initially degraded at 281°C and had a second stage at 396°C (Figure 6a) and a maximum peak (DTG) of 377°C, with a final mass after carbonization of 10% at a temperature of 450°C (Figure 6b). Because of its high density, it is possible that a higher temperature was required to decompose the material until combustion. In general, both species can be used in 3D printers using FDM method, with recommended temperature for PLA filament, which is 200°C to 210°C.
3.6 Fourier Transform Infrared Spectroscopy (FTIR) The vibrational spectra of the printed PLA, composites, and biomass (sawdust powder) are presented in Figure 6c and Figure 6d. Overall, chemical interactions between the polymer and the sawdust are suggested by the observed spectra. The molecular vibrations associated with pure PLA were more intense, while the peaks corresponding to the N. rubra composite were less intense compared to Z. racemosa. The biomass peaks for both species exhibited similar characteristics, with minor variations between them. A prominent biomass band at 3332 cm−1 indicates OH stretching, typically related to hydroxyl groups in cellulose[27,28] This particular region is notably absent or significantly diminished in the composites of both Z. racemosa and N. rubra, suggesting interaction or masking by the PLA matrix. The peaks at 2996 cm−1 and 2918 cm−1 in the samples, 7/10
Bremgartner, J. L., Santos, J., Manzato, L., Bremgartner, V., & Nascimento, C. C.
Figure 6. Sample characterization. (a) TGA; (b) DTG; (c) FTIR of PLA, N.rubra, Z.racemosa. (d) FTIR of sawdust powder from wood (biomass) of N. rubra and Z.racemosa.
and 2914 cm−1 and 2855 cm−1 in the biomass, represent the CH stretching of methyl and methylene groups, which are characteristic of the cellulose, lignin, and hemicellulose content in lignocellulosic materials[22,28,29]. These bands were observed with less intensity in the Z. racemosa composite (Zr/OCB). In the sawdust powder, the peak around 1729 cm−1 is associated with the carbonyl C=O group in hemicellulose[27] appearing more prominent in N. rubra biomass. For the printed samples, the intense band at 1744 cm−1 corresponds to the carbonyl C=O stretching of the lactide group in PLA[22]. The band at 1602 cm−1 in the sawdust spectra corresponds to water absorption[30]. In biomass, the band at 1416 cm−1 are related to lignin and xylan due to CH3 bending vibrations[31]. In the printed samples, the bands between 1446 cm−1 and 1349 cm−1 correspond to bending vibrations CH3[22]. In biomass, the band at 1319 cm−1 is attributed to deformations in the C—H bonds found in cellulose and hemicellulose[27]. The band at 1233 cm−1 is associated with the C—O present in cellulose, hemicellulose, or lignin[27,29]. A prominent peak observed at 1021 cm−1 is attributed to the C—O, C—C or C—OH, characteristic of cellulose and hemicellulose[32]. These bands mentioned previously are more accentuated in the N. rubra composite, suggesting a higher holocellulose content in this species compared to Z. racemosa. Based on these results, it is hypothesized that the greater workability observed for Z. racemosa during extrusion is likely due to its specific fiber characteristics and closed pores, in addition to residual lignin content after degradation, rather than being significantly affected by its holocellulose content. This is because wood fibers generally require high temperatures for degradation[33]. In the printed samples, the region from 1185 cm−1 to 1032 cm−1 encompasses spectra typically classified as C—O—C stretch[22]. 8/10
The band 890 cm−1 is associated with the glycosidic vibration characteristic of the cellulose structure[31]. Lastly, the band at 864 is equivalent to the vibration C—COO and 745 cm−1 is associated with skeletal vibrations of methylene groups[22].
4. Conclusions This study demonstrated the feasibility of producing 3D printing filaments from PLA combined with Amazonian wood waste (from N. rubra and Z. racemosa) and Brazil nut oil (BNO) as a natural binder. Despite the low proportion of wood (4% wt), this research provided an alternative for utilizing Amazonian wood waste, both its natural and diverse colors, adding value to discarded materials and promoting sustainable, biodegradable, and non-toxic 3D bioproducts. Furthermore, it integrates the principles of the circular economy, differentiating itself in the market. Mechanically, while the tensile strength (TS) and compressive strength (CS) of the composites decreased compared to pure PLA, the flexural properties, especially the Modulus of Elasticity (MOE), showed an increase of 153% and 155% for N. rubra and Z. racemosa, respectively. These enhancements suggest that wood fibers, even at low concentrations, can positively influence the elastic performance of printed parts. Z. racemosa provided greater thermal stability to the composite due to its chemical composition. FTIR analysis showed no formation of new chemical bonds, but suggested good compatibility between PLA and the sawdust, corroborated by SEM images. The combination of Amazonian wood waste and PLA presents a promising sustainable alternative for the development of biocomposite filaments for 3D printing. Polímeros, 36(2), e20260021, 2026
Innovations in sustainable additive manufacturing: PLA, Amazon wood waste, Brazil nut oil
5. Author’s Contribution • Conceptualization – Jackeline Lira Bremgartner. • Data curation – Jackeline Lira Bremgartner. • Formal analysis – Jackeline Lira Bremgartner. • Funding acquisition - Jackeline Lira Bremgartner; Lizandro Manzato; Joaquim dos Santos. • Investigation – Jackeline Lira Bremgartner. • Methodology – Jackeline Lira Bremgartner; Vitor Bremgartner; Claudete Catanhede do Nascimento; Lizandro Manzato; Joaquim dos Santos. • Project administration – Jackeline Lira Bremgartner; Joaquim dos Santos; Lizandro Manzato. • Resources – Jackeline Lira Bremgartner; Lizandro Manzato. • Software – Jackeline Lira Bremgartner; Vitor Bremgartner; Lizandro Manzato. • Supervision – Jackeline Lira Bremgartner; Joaquim dos Santos; Lizandro Manzato. • Validation – Jackeline Lira Bremgartner; Vitor Bremgartner. • Visualization – Jackeline Lira Bremgartner. • Writing – original draft – Jackeline Lira Bremgartner; Vitor Bremgartner. • Writing – review & editing – Jackeline Lira Bremgartner; Joaquim dos Santos; Lizandro Manzato; Vitor Bremgartner; Claudete Catanhede do Nascimento.
6. Acknowledgements This work has the following support: Coordination for the Improvement of Higher Education Personnel (CAPES) and the National Council for Scientific and Technological Development (CNPq); Postgraduate Program in Tropical Forest Sciences (CFT/INPA); Laboratory of Synthesis and Characterization of Nanomaterials (LSCN), member of the National System of Nanotechnology Laboratories (SisNANO); Laboratory of Wood Artifacts Engineering (LEAM/INPA), Laboratory of Anatomy and Wood Identification (LAIM/INPA); Institute for Technological Development (INDT); Mechanical Testing Laboratory (LEMAS/IFAM); Multiuser Center for Analysis of Biomedical Phenomena of the State University of Amazonas (CMABio/UEA).
7. References 1. Hidalgo-Carvajal, D., Muñoz, Á. H., Garrido-González, J. J., Carrasco-Gallego, R., & Montero, V. A. (2023). Recycled PLA for 3D printing: a comparison of recycled PLA filaments from waste of different origins after repeated cycles of extrusion. Polymers, 15(17), 3651. https://doi.org/10.3390/polym15173651. PMid:37688276. 2. Khan, M. Z. R., Srivastava, S. K., & Gupta, M. K. (2020). A state-of-the-art review on particulate wood polymer composites: processing, properties and applications. Polymer Testing, 89, 106721. https://doi.org/10.1016/j.polymertesting.2020.106721. 3. Das, A. K., Agar, D. A., Rudolfsson, M., & Larsson, S. H. (2021). A review on wood powders in 3D printing: processes, properties and potential applications. Journal of Materials Polímeros, 36(2), e20260021, 2026
Research and Technology, 15, 241-255. https://doi.org/10.1016/j. jmrt.2021.07.110. 4. Song, Y., Li, Y., Song, W., Yee, K., Lee, K.-Y., & Tagarielli, V. L. (2017). Measurements of the mechanical response of unidirectional 3D-printed PLA. Materials & Design, 123, 154-164. https://doi.org/10.1016/j.matdes.2017.03.051. 5. Kariz, M., Sernek, M., & Kuzman, M. K. (2016). Use of wood powder and adhesive as a mixture for 3D printing. Holz als Roh- und Werkstoff, 74(1), 123-126. https://doi.org/10.1007/ s00107-015-0987-9. 6. Le Duigou, A., Castro, M., Bevan, R., & Martin, N. (2016). 3D printing of wood fibre biocomposites: from mechanical to actuation functionality. Materials & Design, 96, 106-114. https://doi.org/10.1016/j.matdes.2016.02.018. 7. Singh, T., Patnaik, A., Ranakoti, L., Dogossy, G., & Lendvai, L. (2022). Thermal and sliding wear Properties of Wood Waste-Filled Poly(Lactic Acid) Biocomposites. Polymers, 14(11), 2230. https://doi.org/10.3390/polym14112230. PMid:35683903. 8. Huang, Y., Löschke, S., & Proust, G. (2021). In the mix: the effect of wood composition on the 3D printability and mechanical performance of wood-plastic composites. Composites Part C: Open Access, 5, 100140. https://doi.org/10.1016/j. jcomc.2021.100140. 9. Kariz, M., Sernek, M., Obućina, M., & Kuzman, M. K. (2018). Effect of wood content in FDM filament on properties of 3D printed parts. Materials Today. Communications, 14, 135-140. https://doi.org/10.1016/j.mtcomm.2017.12.016. 10. Tao, Y., Wang, H., Li, Z., Li, P., & Shi, S. Q. (2017). Development and application of wood flour-filled polylactic acid composite filament for 3D printing. Materials (Basel), 10(4), 339. https://doi.org/10.3390/ma10040339. PMid:28772694. 11. Pereira, D., Santos, D., Vedoveto, M., Guimarães, J., & Veríssimo, A. (2010). Fatos florestais da Amazônia 2010. Imazon. Retrieved in 2025, July 16, from https://imazon.org. br/publicacoes/fatos-florestais-da-amazonia-2010/ 12. Andrade, K. D. C., Santos, A. P. F., Emmert, F., Santos, J., Lima, A. J. N., & Higuchi, N. (2022). Volumetric yield coefficient: the key to regulating virtual credits for Amazon wood. Acta Amazonica, 53(1), 1-8. https://doi.org/10.1590/1809-4392202101602. 13. Nascimento, J. C. (2021). Influência da classificação de toras, características anatômicas e dendrométricas e o tempo de espera entre o corte e o desdobro no rendimento volumétrico da Nectandra rubra (Mez) C. K. Allen (Master’s thesis). Instituto Nacional de Pesquisas da Amazônia, Manaus. 14. Esteves, L. L. (2018). A influência de óleos vegetais sobre a degradação e propriedades do polipropileno reciclado (Master’s thesis). Instituto Politécnico, Universidade do Estado do Rio de Janeiro, Nova Friburgo. 15. Carvalho, A. L. S., Martelli, M. C., Nascimento, S. C. C., & Brasil, D. S. B. (2022). Brazil Nut oil: extraction methods and industrial applications. Research, Social Development, 11(4), e29511427256. https://doi.org/10.33448/rsd-v11i4.27256. 16. Pereira, E., Ferreira, M. C., Sampaio, K. A., Grimaldi, R., Meirelles, A. J. A., & Maximo, G. J. (2019). Physical properties of Amazonian fats and oils and their blends. Food Chemistry, 278, 208-215. https://doi.org/10.1016/j.foodchem.2018.11.016. PMid:30583364. 17. Narlıoğlu, N., Salan, T., & Alma, M. H. (2021). Properties of 3D-printed wood sawdust-reinforced PLA composites. BioResources, 16(3), 5467-5480. https://doi.org/10.15376/biores.16.3.5467-5480. 18. Yang, T.-C., & Yeh, C.-H. (2020). Morphology and mechanical properties of 3d printed wood fiber/polylactic acid composite parts using Fused Deposition Modeling (FDM): the effects of printing speed. Polymers, 12(6), 1334. https://doi.org/10.3390/ polym12061334. PMid:32545359. 9/10
Bremgartner, J. L., Santos, J., Manzato, L., Bremgartner, V., & Nascimento, C. C. 19. Yang, T.-C. (2018). Effect of extrusion temperature on the physico-mechanical properties of unidirectional Wood Fiber-Reinforced Polylactic Acid Composite (WFRPC) components using fused deposition modeling. Polymers, 10(9), 976. https://doi.org/10.3390/polym10090976. PMid:30960901. 20. Ferreira, G. C., & Hopkins, M. J. G. (2004). Manual de identificação botânica e anatômica. Belém: Embrapa Amazônia Oriental. 21. Sousa, M. H., Magliano, M. M., Camargos, J. A. A., & Souza, M. R. (2002). Madeiras tropicais brasileiras. Brasília: Edições IBAMA. 22. Santana, L., Alves, J. L., Sabino Netto, A. C., & Merlini, C. (2018). Estudo comparativo entre PETG e PLA para Impressão 3D através de caracterização térmica, química e mecânica. Revista Matéria, 23(4), e-12267. https://doi.org/10.1590/S1517-707620180004.0601. 23. Agaliotis, E. M., Ake-Concha, B. D., May-Pat, A., Morales-Arias, J. P., Bernal, C., Valadez-Gonzalez, A., Herrera-Franco, P. J., Proust, G., Koh-Dzul, J. F., Carrillo, J. G., & Flores-Johnson, E. A. (2022). Tensile Behavior of 3D Printed Polylactic Acid (PLA) based composites reinforced with natural fiber. Polymers, 14(19), 3976. https://doi.org/10.3390/polym14193976. PMid:36235924. 24. Yang, H., Yan, R., Chen, H., Lee, D. H., & Zheng, C. (2007). Characteristics of hemicellulose, cellulose and lignin pyrolysis. Fuel, 86(12-13), 1781-1788. https://doi.org/10.1016/j. fuel.2006.12.013. 25. Figueroa, M. J. M., & Moraes, P. D. (2009). Comportamento da madeira a temperaturas elevadas. Ambiente Construído, 9(4), 157-174. https://doi.org/10.1590/s1678-86212009000400525. 26. Poletto, M., Zattera, A. J., Forte, M. M. C., & Santana, R. M. C. (2012). Thermal decomposition of wood: influence of wood components and cellulose crystallite size. Bioresource Technology, 109, 148-153. https://doi.org/10.1016/j.biortech.2011.11.122. PMid:22306076. 27. Charis, G., Danha, G., & Muzenda, E. (2020). Characterizations of biomasses for subsequent thermochemical conversion: a comparative study of pine sawdust and acacia tortilis. Processes
10/10
(Basel, Switzerland), 8(5), 546. https://doi.org/10.3390/ pr8050546. 28. Barros, S. S. (2020). Síntese e caracterização de nanocelulose a partir da folha de abacaxi (Ananas comosus (L.) Merr.) (Master’s thesis). Faculdade de Tecnologia, Universidade Federal do Amazonas, Manaus. 29. Siriprom, W., Sangwaranatee, N., Herman, K., Chantarasunthon, K., Teanchai, K., & Chamchoi, N. (2018). Characterization and analyzation of the poly (L-lactic acid) (PLA) films. Materials Today: Proceedings, 5(7), 14803-14806. https://doi.org/10.1016/j.matpr.2018.04.009. 30. Abraham, E., Deepa, B., Pothan, L. A., Jacob, M., Thomas, S., Cvelbar, U., & Anandjiwala, R. (2011). Extraction of nanocellulose fibrils from lignocellulosic fibres: a novel approach. Carbohydrate Polymers, 86(4), 1468-1475. https://doi.org/10.1016/j.carbpol.2011.06.034. 31. Manzato, L., Takeno, M. L., Pessoa-Junior, W. A. G., Mariuba, L. A. M., & Simonsen, J. (2018). Optimization of cellulose extraction from jute fiber by box-behnken design. Fibers and Polymers, 19(2), 289-296. https://doi.org/10.1007/s12221-018-1123-8. 32. Raspolli Galletti, A. M., D’Alessio, A., Licursi, D., Antonetti, C., Valentini, G., Galia, A., & Nassi o Di Nasso, N. (2015). Midinfrared FT-IR as a tool for monitoring herbaceous biomass composition and its conversionto furfural. Journal of Spectroscopy, 2015(1), 719042. https://doi.org/10.1155/2015/719042. 33. Abreu, R., No., Lima, J. T., Takarada, L. M., & Trugilho, P. F. (2021). Efeito do tratamento térmico na morfologia das fibras na pirólise da madeira. Wood Science and Technology, 55(1), 95-108. https://doi.org/10.1007/s00226-020-01238-6. Received: Jul. 16, 2025 Revised: Feb. 17, 2026 Accepted: Feb. 20, 2026 Editor-in-Chief: Sebastião V. Canevarolo
Polímeros, 36(2), e20260021, 2026
ISSN 1678-5169 (Online)
https://doi.org/10.1590/0104-1428.0250045
Sorption of phenanthrene by crosslinked polymers with varied monomeric compositions Rafael de Lima Pinto1 , Ezaine Cristina Corrêa Torquato2 , Luciana da Cunha Costa2* , Caroline Felix Carvalho2 and Mônica Regina da Costa Marques Calderari1 Central Analítica Fernanda Coutinho, Instituto de Química, Universidade do Estado do Rio de Janeiro - UERJ, Rio de Janeiro, RJ, Brasil 2 Departamento de Farmácia, Faculdade de Ciências Biológicas e Saúde, Universidade do Estado do Rio de Janeiro - UERJ, Rio de Janeiro, RJ, Brasil
1
*luciana.cunha.costa@uerj.br; luciana.cunha.costa@gmail.com
Abstract Solid-phase extraction is an efficient strategy for preconcentrating several analytes. Studies of the relationship between the monomeric composition of polymers and sorption capacity of polycyclic aromatic hydrocarbons (PAHs) need to be expanded, seeking to contribute to the identification of the most suitable polymers for preconcentrating this pollutant. We selected crosslinked polymers with different monomer compositions for this study. These polymers were prepared by combining divinylbenzene or ethylene glycol dimethacrylate, with several comonomers. The polymers crosslinked with DVB had higher removal efficiency than those crosslinked with EGDMA. At equilibrium, the amount of phenanthrene adsorbed was 0.314 mg g−1 for poly(DVB) and 0.271 mg g−1 for poly(Sty-co-DVB). Poly(DVB) demonstrated a working capacity of 0.152 g cm-3. Notably, complete removal of phenanthrene from the aqueous leachate of drill cuttings was achieved using poly(DVB), indicating that this contaminant was effectively retained by the solid-phase extraction (SPE) column utilizing this polymer. Keywords: drill cuttings, PAHs, phenanthrene, solid phase extraction, styrene-divinylbenzene copolymers. Data Availability: All data supporting the findings of this study are available from the corresponding author upon request. How to cite: Pinto, R. L., Torquato, E. C. C., Costa, L. C., Carvalho, C. F., & Calderari, M. R. C. M. (2026). Sorption of phenanthrene by crosslinked polymers with varied monomeric compositions. Polímeros: Ciência e Tecnologia, 36(2), e20260022. https://doi.org/10.1590/0104-1428.0250045
1. Introduction Polycyclic aromatic hydrocarbons (PAHs) compose a class of ubiquitous compounds present in several environmental compartments and are considered persistent organic pollutants (POPs) [1]. Phenanthrene, along with other polycyclic aromatic hydrocarbons (PAHs) can serve as a marker for assessing petrogenic contamination in drilling waste during oil and gas production processes. Previous studies[2] have reported that phenanthrene is often found in higher concentrations than other PAHs in drill cuttings. Phenanthrene is noteworthy because it ranks fifth in solubility among the 16 priority PAHs. When considering PAHs as indicators of pyrogenic and petrogenic contamination, it’s important to note that their solubility in water is lower than that of naphthalene, which has a high partial vapor pressure, but higher than that of many other PAHs. This indicates that phenanthrene has significant potential to cause harm in aquatic environments. Solid-phase extraction (SPE) is an effective method for separating and concentrating various environmentally important analytes. The hydrophilic-lipophilic balance is essential in determining the composition of SPE cartridge
Polímeros, 36(2), e20260022, 2026
fillings because it enhances the separation efficiency. A classic example of this is the use of SPE C18 and C8 cartridges in both offline SPE and dispersive micro SPE techniques[3]. Crosslinked copolymers are effective sorbent materials for solid-phase extraction (SPE) cartridges. Research indicates that these materials can efficiently remove organic and inorganic pollutants from aqueous media. Their advantages include physical and chemical stability, low monomer cost, the ability to control morphological characteristics such as pore structure and surface area, and ease of regeneration and reuse[4-6]. Several researchers have investigated crosslinked polymers as absorbents for the sorption and pre-concentration of PAHs[6-8]. However, these works do not explore the employment of crosslinked polymers with varied monomeric compositions in detail. Polymeric particles from combining monomers with different polarities can have different morphologies and swelling capacities in aqueous media, resulting in different PAH sorption capacities. This study’s results can contribute to developing polymers with a hydrophilic-hydrophobic balance that is more suitable for SPE.
1/9
O O O O O O O O O O O O O O O O
Pinto, R. L., Torquato, E. C. C., Costa, L. C., Carvalho, C. F., & Calderari, M. R. C. M. We aimed to evaluate the phenanthrene adsorption process by crosslinked polymeric microspheres with varied monomeric compositions. These microspheres, previously prepared according to Torquato et al.[9] were based on divinylbenzene (DVB) or ethylene glycol dimethacrylate (EGDMA) combined with styrene (Sty), 4-vinylbenzyl chloride (VBC), glycidyl methacrylate (GMA) and methacrylic acid (MAA). The particles were evaluated for their ability to retain phenanthrene in water through continuous flow tests (column). Particles with higher sorption capacity were assessed in terms of their equilibrium and adsorption kinetics. These polymers were also evaluated in initial studies of sorption of aqueous leachate from offshore oil drilling cuttings, enriched with phenanthrene.
2. Materials and Methods 2.1 Selection of the polymers Ten polymeric microspheres were selected for this work (Table 1). These particles were synthesized by aqueous suspension polymerization, according to a previous study[9]. The organic phase was composed of 0.12 mol of comonomer (Sty, VBC, GMA or MAA), 0.18 mol of crosslinker (DVB or EGDMA), AIBN (1% mol/mol related to monomers), n-heptane (150% of dilution degree). The aqueous phase was composed of distilled water (200 mL), PVA (2% w/v of water volume), and NaCl (3% w/v of water volume). The polymerization was carried out under continuous stirring at 200 rpm at 80 °C for 24 h. The microspheres were filtered and washed with hot distilled water, ethanol, and acetone. The particles were dried at 60 °C for 24 hours[9]. Table 1 and Table 2 show data of surface area pore volume, and pore diameter of the particles selected for this study[9].
Table 1S and Table 2S (supplementary material) present data of swelling degree in water and swelling degree in methanol of these particles.
2.2 Preliminary experiments The concentration of phenanthrene in the solutions was quantified using a fluorescence spectrophotometer (Agilent Technologies Cary Eclipse), equipped with a xenon lamp. The main parameters for obtaining the emission spectrum are described in Table 3S. The analytical curve was prepared using phenanthrene standard solution and ultrapure water (1 mg L-1). This value was determined considering the solubility limit of phenanthrene (1.1 mg L-1). Phenanthrene solubilization was achieved by sonication of the solution. The statistical study on the method’s linearity recommended by the INMETRO DOQCGCRE-008 guide[10]. Quantification (QL) and detection (DL) limits were calculated considering the lowest concentration (0.2 mg L-1) of the validated analytical curve[10]. The polymers were submitted to pretreatment with methanol and distilled water (10 mL) before the sorption experiments.
2.3 Batch sorption experiment 2.3.1 Preliminary adsorption tests Preliminary adsorption tests were carried out to verify the feasibility and effectiveness of phenanthrene sorption using crosslinked polymers with different monomeric compositions as adsorbents. The experiments were conducted in batches obtained from the dispersion of 15 mg of polymers in test tubes containing 5 mL of phenanthrene solution (1.0 mg L-1). The tubes were placed on a Kline shaker (NT150, Novatecnica, Brazil) and left under mechanical agitation (200 rpm) for 30 min at room temperature.
Table 1. Data of surface area, pore volume, pore diameter of the polymers based on DVB[9].
SBET (m2 g‒1) VpBJH (cm3 g‒1) D (Å)
Poly(DVB) 447.9 0.91 105.1
Poly(VBC-co-DVB) 29.4 0.10 120.9
Poly(GMA-co-DVB) 19.9 0.15 193.8
Poly(MAA-co-DVB) 60.7 0.07 69.9
Poly(Sty-co-DVB) 175.2 0.62 174.1
Table 2. Data of surface area, pore volume, pore diameter of the polymers based on EGDMA [9]
SBET (m2 g‒1) VpBJH (cm3 g‒1) D (Å)
2/9
Poly(EGDMA) Poly(VBC-co-EGDMA) Poly(GMA-co-EGDMA) 7.77 6.28 9.34 0.03 0.03 0.03 290.97 256.21 113.41
Poly(MAA-co-EGDMA) 7.45 0.03 170.70
Poly(Sty-co-EGDMA) 61.46 0.04 30.58
Polímeros, 36(2), e20260022, 2026
Sorption of phenanthrene by crosslinked polymers with varied monomeric compositions The phenanthrene concentration was measured using a fluorescence spectrophotometer (Cary Eclipse, Agilent, USA), and the excitation and emission wavelengths were 250 nm and 364 nm, respectively. The percentage of phenanthrene removed from the aqueous solution by the polymers was determined according supplementary material (Table 4S)[11]. 2.3.2 Sorption capacity The polymers with the highest sorption capacities according to the preliminary tests (test 2.3.1) were selected for this study. A total of 0.2 g of these polymers was placed in contact with 40 mL of phenanthrene solution at varying concentrations (0.2 to 1.0 mg L−1). The flasks were then placed in a shaker incubator (model NT712, Novatecnica, Brazil) set at 25 °C and 200 rpm for 30 minutes. The concentration of phenanthrene in the solution was measured using spectrofluorimetry. The adsorption capacity (qe, mg g−1) of phenanthrene was calculated using equation described on supplementary material (Table 4S)[11]. Adsorption equilibrium data were analyzed using Langmuir and Freundlich models (in their linearized versions)[11,12] (presented in Table 5S) (supplementary material). 2.3.3 Kinetic study This study focused exclusively on polymers with higher sorption capacities, in which 0.15 g of each polymer was placed in contact with 5 mL of phenanthrene solution at a concentration of 1.0 mg L-1. The flasks containing the mixtures were kept in a shaker incubator at 25 °C at 200 rpm. Samples were collected at specific time intervals (1, 10, 30, 60, 120, 180, 240, and 1440 minutes), and the concentration of phenanthrene in the solution was measured by spectrofluorimetry. All experiments were conducted in triplicate. Kinetic data were analyzed using kinetic models of pseudo-first order, pseudo-second order, and Elovich, as well as diffusion models such as external diffusion, Weber-Morris, and Urano-Tachikawa intraparticle diffusion, presented in their linearized forms in Table 5S[11,12].
2.5 Study involving leachate from drill cuttings This study used a carbonate drill cutting sample containing water-based drilling fluid. An aqueous leachate derived from this sample was prepared according to Soares et al.[2]. The drill cutting solution (1 mg L-1) (25 mL) was percolated through a polymer-packed column using a solid-phase extraction (SPE) system connected to a vacuum pump. The solution eluted from the column was analyzed by fluorimetry to determine the adsorption efficiency on the polymer. After this analysis, the column was eluted with acetonitrile. The eluate was evaporated using a rotary evaporator (R-124, BUCHI, Switzerland). The resulting residue was transferred to a vial and reconstituted in 1 mL of hexane for subsequent gas chromatography analysis. The chromatographic conditions were described on work of Soares et al.[2].
3. Results and Discussion The supplementary material details the construction of the analytical curve (Figure 2S), as well as the limits of linearity, detection, and quantification.
3.1 Preliminary adsorption study The preliminary sorption tests (Figure 1) were conducted in batches, according to batch, by item 2.3.1, using the ten polymers defined in Tables 1 and 2. This study employed 5 mL of phenanthrene solution (1.0 mg L-1) and 0.15 g of polymeric particles. Based on the results of the sorption capacity of phenanthrene, it was possible to assume that the sorption efficiency of the polymers was the result of the contribution of adsorption phenomena, favored by materials with larger surface areas and pore volumes, allied to hydrophobic partitioning, based on hydrophobic interactions between adsorbent and adsorbate. The DVB polymer showed the best phenanthrene removal efficiency (99.9%) compared to the other particles.
2.4 Column adsorption study This study utilized a polypropylene column with internal diameter of 0.47 cm and a height of 7.53 cm, packed with 15 mg of polymer. The bed was fixed and wrapped with glass wool. Peristaltic pump (TE-BP-01, Tecnal, Brazil) was connected to the column’s upper inlet to control the feed flow rate (Figure 1S, supplementary material). The column was conditioned with methanol (10 mL) and ultrapure water (10 mL). Subsequently, phenanthrene solutions (1.0 mg L-1) were pumped through the column at a flow rate of 10 mL min-1. Aliquots of 5 mL were collected at specific intervals while maintaining a constant flow throughout the process. The collected aliquots were analyzed by spectrofluorimetric. The breakthrough curve was obtained by plotting the ratio of the phenanthrene concentration in the outlet/and inlet solution (C/C0) versus the volume of solution passed through the column. The data obtained through this rupture curve were used to calculate the adsorption work capacity, CW (g cm-3) and total adsorption capacity, CT (g cm‒3)[11,12]. These equations are described on Table 4S. Polímeros, 36(2), e20260022, 2026
Figure 1. Phenanthrene capacity removal by crosslinked polymers. Initial phenanthrene concentration: 1.0 mg L-1, Temperature: 25 °C. DVB: divinylbenzene, EGDMA: ethylene glycol dimethacrylate, Sty: styrene, VBC: 4-vinylbenzyl chloride, GMA: glycidyl methacrylate, MAA: methacrylic acid. 3/9
Pinto, R. L., Torquato, E. C. C., Costa, L. C., Carvalho, C. F., & Calderari, M. R. C. M. This polymer had the highest surface area and pore volume, which probably favored the diffusion of this analyte through this material’s internal structure and consequently the analyte’s adsorption process. Poly(GMA-co-DVB), poly(MAA-coDVB), poly(Sty-co-DVB), and poly(Sty-co-EGDMA) had higher sorption capacity of phenanthrene than 90%. Poly(Sty-co-DVB) showed 175 m2 g-1 of BET surface area, poly(MAA-co-DVB) and poly(Sty-co-EGDMA) also showed high surface areas (around 60 m2 g-1). Poly(GMA-co-DVB) had a surface area of around 20 m2 g-1, but these particles had higher pore volumes and pore diameters, which can also favor the phenanthrene sorption. It was not possible to establish a correlation between the swelling capacity of the polymers in water and methanol (Table 1S and Table 2S, supplementary material) and the sorption capacity of phenanthrene. The swelling capacity of polymers in water or methanol ranged from 3 to 9%. This low degree of swelling may help explain the lack of correlation between swelling capacity and sorption capacity of phenanthrene by these particles. The low degree of swelling of the polymers in these solvents might have been related to the high crosslinking degree of these polymers. The content of divinyl monomer (DVB or EGDMA) in the monomeric mixture during polymerization was 60%. Most particles had hydrophobic surfaces, with contact angles varying from 90° to 150° (Table 1S and Table 2S). Poly(VBC-co-DVB) had a contact angle of 89.3 º, indicating that this material has a hydrophilic surface. This polymer presented a lower phenanthrene sorption capacity than the other DVB-based polymers, indicating that the hydrophilicity of this surface did not favor the sorption of phenanthrene. According to Fujiwaraet al.[13], “the solubility parameter, a physical property representing the cohesion energy density of a substance, is useful for evaluating the compatibility, wettability, and cohesiveness or dispersibility of substances”. According to Bielicka-Daszkiewicz et al.[14] Hansen solubility parameters can be used to analyze the interactions in sorbent–analyte–eluent systems in solid phase extraction. The sorption of phenanthrene by the polymers can also be attributed to the reversible hydrophobic partitioning between phenanthrene molecules and the hydrophobic surfaces. This partitioning can be understood by analyzing the Hansen solubility parameters of the adsorbent and adsorbate. The values of the Hansen solubility parameters (δ) of phenanthrene and monomers used in the preparation of microspheres are shown in Table 6S and Table 7S (supplementary material). The Hansen solubility parameter of phenanthrene had a significantly greater contribution of dispersion forces (δd) and a lower contribution of dipole-dipole forces (δp)[15]. The Hansen solubility parameter of the DVB crosslinker also presented a high contribution of δd. On the other hand, the solubility parameter of EGDMA crosslinker indicated a low contribution of δd and a high contribution of δp. The DVBbased polymers generally presented a greater phenanthrene sorption capacity than those crosslinked with EGDMA, which can be related to dispersion interactions between the adsorbent and adsorbate. According to Qin et al.[16], the phenomenon of adsorption of phenanthrene molecules by polystyrene is driven by hydrophobic interactions such as van der Waals forces and mainly by π-π interactions. 4/9
It is noteworthy that the addition of a monomer containing polar groups (such as an epoxide ring, carboxyl and chloromethyl groups) to the polymers based on DVB caused a decrease in the removal efficiency of phenanthrene, which can be attributed to a reduction of dispersion forces accompanied by increased contributions of dipole-dipole forces (δp) and hydrogenbonding interactions (δh) on these adsorbents. When analyzing the polymers crosslinked with EGDMA, we observed that particles prepared with Sty comonomer were more efficient in removing phenanthrene from water. This can be explained since phenanthrene, and Sty had more significant contributions to the dispersion forces. On the other hand, the combination of EGDMA with the monomers GMA and MMA generated particles with a lower phenanthrene sorption capacity. These monomers have high contributions of dipole-dipole forces (δp) and hydrogen-bonding interactions, and consequently, a lower contribution of dispersion forces. The following order of phenanthrene sorption was established: poly(DVB), poly(Sty-co-EGDMA), poly(Styco-DVB), poly(MAA-co-DVB), poly(GMA-co-DVB), poly(VBC-co-DVB), poly(VBC-co- EGDMA), poly(EGDMA), poly(MAA-co- EGDMA), poly(GMA-co- EGDMA). We selected poly(DVB) and poly(Sty-co-DVB) for the subsequent steps. This choice was made considering the phenanthrene sorption capacity and the mechanical stability of these materials. Combining monomers with different polarities such as GMA with DVB and, MAA and DVB generated brittle particles (Figure 3S, supplementary material). Combining EGDMA with most monomers also generated brittle particles (Figure 4S, supplementary material). The polymerization reaction occurs in the oil phase of aqueous suspension polymerization, within the monomer droplets. When these monomers are more polar, maintaining the stability of the suspension becomes more difficult, compromising the mechanical stability and sphericity of the particles generated.
3.2 Batch adsorption experiments 3.2.1 Adsorption equilibrium study Data on the variation of the sorption capacity (qe) as a function of the variation of the phenanthrene concentration were fitted to both the Langmuir and the Freundlich models. The phenanthrene adsorption isotherms on poly(DVB) and poly (Sty-co-DVB) (Figure 5S, supplementary material) showed that, as expected, the adsorption capacity of both polymers increased significantly as the phenanthrene concentration increased. The Langmuir equation assumes that adsorption occurs on the surface of the solid and that the surface is covered by a monolayer. According to Dotto et al.[11], the Langmuir theory assumes that adsorption occurs at specific and homogeneous sites on the surface of the adsorbent. Each site is responsible for the adsorption of only one analyte molecule, and no additional adsorption can occur. The Langmuir isotherm’s separation factor (RL) provides important information. The RL data for poly(DVB) and poly(Sty-co-DVB) were 0.93 and 0.94, respectively, indicating a favorable sorption process (Dotto et al.)[11]. The Freundlich model assumes that multilayer adsorption is a process on a heterogeneous surface. In other words, the Freundlich isotherm is used for systems with heterogeneous surfaces, where multilayer adsorption occurs along with interaction between the adsorbate molecules[11]. Polímeros, 36(2), e20260022, 2026
Sorption of phenanthrene by crosslinked polymers with varied monomeric compositions The Freundlich model was a better fit for the observed adsorption than the Langmuir model (Table 3), indicating that the phenanthrene adsorption process on the surface of poly(DVB) and poly(Sty-co-DVB) exhibited multilayer behavior. The magnitude of the exponent 1/n between 0 and 1 and values of n greater than 1 indicate favorable conditions for adsorption. 3.2.2 Adsorption kinetics study Sorption equilibrium of phenanthrene was reached after approximately 30 minutes and the qt values were 0.313 ± 0.002 and 0.273 ± 0.001 (mg g-1) for the poly(DVB) and poly(Sty-co-DVB), respectively (Figure 2) and Table 7S.
Pseudo-first-order (Lagergren), pseudo-second-order, and Elovich models were chosen to study the sorption of phenanthrene by polymers. In addition, the sorption mechanism was also studied employing diffusional kinetic models such as external diffusion, Weber-Morris intraparticle diffusion, and Urano-Tachikawa intraparticle diffusion. Through the linearization of the pseudo-firstorder model (Lagergren), we ploted the graph of ln(qe-qt) versus time (Figure 6S, supplementary material). From the data obtained from the graph, the values of k1 and qe,calc were determined based on the data obtained from the graph. These parameters are shown in Table 4. The coefficients of determination R2 ranged from 0.879 to 0.996.
Figure 2. (a) Adsorption kinetics and (b) Removal efficiency of phenanthrene by polymers. Initial phenanthrene concentration: 1.0 mg L-1, Temperature: 25 °C.
Table 3. Isothermal parameters for adsorption of phenanthrene on poly(DVB) and poly(Sty-co-DVB). Isotherm models Coefficients R2 KL (L mg−1) RL qmax (mg g−1)
Langmuir Polymers poly(DVB) poly(Sty-co-DVB) 0.9362 0.3648 0.07 0.07 0.9364 0.9432 277.78 263.16
R2 KF (mg g−1) n
poly(DVB) 0.9998 17.68 1.03
Freundlich poly(Sty-co-DVB) 0.998 16.94 1.02
KL: Langmuir constant, RL: Langmuir isotherm’s separation factor, KF: Freundlich constant, 1/n: heterogeneity factor.
Table 4. Parameters of reaction kinetic models for the adsorption of phenanthrene on poly(DVB) and poly(Sty-co-DVB). Models
Pseudo-first order Polymers Coef. Poly Poly (DVB) (Sty-co-DVB) -0.252 -0.231 a -1.980 -2.328 b 0.949 0.879 R2 0.252 0.231 k1 (min‒1) 0.098 qe,calc (mg g‒1) 0.138 qe,exp (mg g‒1) 0.311 ± 0.001 0.272 ± 0.001
Pseudo-second order Polymers Coef. Poly Poly (DVB) (Sty-co-DVB) 3.187 3.691 a 1.699 1.741 b 0.995 0.996 R2 7.825 k2 (g mg‒1 min‒1) 5.976 0.271 qe,calc (mg g‒1) 0.314 0.313 ± 0.002 0.273 ± 0.001 qe,exp (mg g‒1) 0.574 h (mg g‒1 min‒1) 0.589
Elovich Polymers Coef. Poly Poly (DVB) (Sty-co-DVB) 2.829 2.486 a 0.197 0.172 b 0.974 0.951 R2 α (mg g‒1 min‒1) 2.829 2.486 β (mg g‒1) 20.704 23.697
a: angular coefficient, b: linear coefficient, k1: pseudo-first-order constant; qe,calc: theorical adsorption capacity; qe,exp: experimental adsorption capacities; k2: pseudo-second-order constant; h: initial adsorption rate; α: initial adsorption rate; β: desorption constant.
Polímeros, 36(2), e20260022, 2026
5/9
Pinto, R. L., Torquato, E. C. C., Costa, L. C., Carvalho, C. F., & Calderari, M. R. C. M. The value of the calculated maximum adsorption capacity at equilibrium (qe,calc) according to the equation representing the pseudo-first order model disagreed with the values of the maximum experimental adsorption capacities (qe,exp) for phenanthrene solutions with initial concentrations of 1.0 mg L-1. According to Crini et al.[17], “this model assumes that the rate of change of solute uptake with time is directly proportional to the difference in saturation concentration and the amount of solid uptake”. According to Vareda[18:5], the equation used to describe this model “is an adaptation from reaction kinetics of homogenous systems, which means that this model is a surface reaction model and suggests occupation of one active surface site by the adsorbate”. On the other hand, the pseudo-second order model enabled us to obtain better results. The pseudo-second order kinetic constant (k2) and the qecalc were obtained from constructing the graph of t/qt versus time (Figure 6S). The values of the R2 coefficients were 0.995 and 0.996 for poly(DVB) and poly(Sty-co-DVB), respectively. Furthermore, the values of qecalc agreed with qeexp. The qecalc values for phenanthrene adsorption by poly(DVB) and poly(Sty-co-DVB) obtained in this work are 0.314 and 0.271 mg g-1, respectively. These results indicate that the pseudo-second order mechanism is the best predictor of the adsorption process for both adsorbents. The pseudo-second-order rate expression is used to describe chemisorption involving valence forces through the sharing or exchange of electrons between the adsorbent and adsorbate as covalent forces, while ion exchange, according to second-order kinetics concern the available sites[19,20]. As commented before, “this model assumes that the sorption kinetics is determined by a chemical reaction between sorbent and sorbate, while the properties of sorbent and conditions of the medium influence the adsorption kinetics. The adsorption process depends on the concentration of solute molecules in the solution and the number of unoccupied sites in the sorbent. In contrast, desorption relies on the number of occupied sites in the sorbent[12]. Figure 6S plots the Elovich equation for the same experimental data. By employing this model, it was possible to obtain a linear relationship between qt versus lnt over the adsorption period, obtaining R2 coefficients of 0.974 and 0.951 for the poly(DVB) and poly(Sty-co-DVB), respectively. These coefficient values for the Elovich equation are lower than those obtained using the pseudo-second order model, indicating that the Elovich model cannot be used to predict the adsorption kinetics of phenanthrene on polymers. The Elovich equation is commonly used to describe the adsorption of gases on solids[19].
Using the linear form of the Weber-Morris intraparticle diffusion model, the curve graph was constructed by plotting qt versus time1/2 (Figure 7S, supplementary material). We then determined the intraparticle diffusion constant (kid) from the data obtained from the graph (Table 5). It is possible to observe a linear relationship between qt and time1/2 using the equation representing the Weber-Morris model (Figure 7S, supplementary material). The R2 values were 0.914 and 0.863 for the poly(DVB) and poly(Sty-co-DVB), respectively. As can be seen, the line does not pass through the origin, indicating some degree of boundary layer control and that intraparticle diffusion is not the only step. Other processes can also control the adsorption rate[19]. The results showed that these graphs can present multilinearity, indicating that the adsorption occurs in two or more stages. In the Urano-Tachikawa intraparticle diffusion model, the adsorption rate is minimal and independent of stirring speed, so external diffusion is not relevant compared to the overall adsorption rate[20]. Through the linearization of the equation that represents this model, it is possible to construct the graph of the curve by plotting ‒log[1 ‒ (qt/qe)2] versus time (Figure 7S, supplementary material). Average particle diameter (d) values for poly(DVB) and poly(Sty-co-DVB) are 5.93 10‒3 and 2.84x10‒2 cm, respectively. The intra-particle diffusion coefficient of Urano-Tachikawa (Di) was obtained from the slope value of the graph in Figure 7S. The data are presented in Table 5. The R2 coefficients for the poly(DVB) and poly (Sty-co-DVB) were 0.956 and 0.906, indicating a disagreement between this model and the data obtained experimentally.
3.3 Column adsorption experiments In this stage of the study, we evaluated the performance of poly(DVB) in a column experiment aimed at constructing the breakthrough curve under controlled column feed flow conditions. As detailed in section 2.4, the study involved the elution of 23.8 liters of phenanthrene solutions at a concentration of 1.0 mg/L, which had been quantitatively analyzed using spectrofluorimetry. This was conducted through a column packed with 15 mg (approximately 0.07 cm3) of poly(DVB). During the experiment, several aliquots were collected with the flow rate maintained at approximately 10 mL min-1. The column was fed with the phenanthrene solutions until total saturation was reached, which is defined as the point where the concentration of phenanthrene entering the column (C0) was nearly equal to the concentration of phenanthrene exiting the column (C), resulting in a ratio (C/C0) of approximately 0.1.
Table 5. Parameters of the diffusional kinetic models for the adsorption of phenanthrene in poly(DVB) and poly(Sty-co-DVB). Models Coef. a b R2 kf (cm s‒1)
External diffusion Poly (DVB) -0.004 -0.831 0.948
Polymers Poly (Sty-co-DVB) -0.004 -1.023 0.880
Coef.
a b R2 kid (mg g‒1 min-1/2)
Intraparticle diffusion (Weber-Morris) Polymers Poly Poly (DVB) (Sty-co-DVB) 0.048 0.042 0.161 0.142 0.914 0.863 0.048 0.042
Coef.
a b R2 Di (10‒8) (cm2 s‒1)
Intraparticle diffusion (Urano-Tachikawa) Polymers Poly Poly (DVB) (Sty-co-DVB) 0.002 0.002 0.093 0.148 0.956 0.906 3.59 77.7
a: angular coefficient, b: linear coefficient, kid : intraparticle diffusion rate constant; Di ‒ sum of diffusion in the pores and in the film.
6/9
Polímeros, 36(2), e20260022, 2026
Sorption of phenanthrene by crosslinked polymers with varied monomeric compositions Analyzing the variation of this ratio concerning the volume of the eluted solution provided insights into the adsorption capacity of the polymer. It facilitated the construction of the breakthrough curve (Figure 8S, supplementary material). When analyzing the rupture curve graph profile, we observed that the removal of phenanthrene by the poly(DVB) was highly effective in the initial stages of the elution process. Subsequently, the phenanthrene removal efficiency decreased because of the progressive saturation of available active sites on the surface of the adsorbent material. When approximately 11.8 L of solution was eluted, the phenanthrene concentration levels reached the saturation plateau, indicated on the curve by the flattening trend. At this point, the C/C0 ratio was close to 0.7. Then, we continued to be feed to the column, and observed that after the elution of 23.8 L, there was no significant change in the C/C0 ratio, confirming that the column had already reached the saturation point. The highlighted data indicates the point where saturation occurred. The calculated adsorption working capacity (CW) and total adsorption capacity (CT) for the poly(DVB) were 0.152 g cm-3 and 0.0289 g cm-3, respectively.
3.4 Phenanthrene recovery test in leachate from drill cuttings The concentration of phenanthrene in the drill cuttings sample in the recovery test was quantified by GC-FID using a calibration curve with good linearity (R2 = 0.9995) in the concentration range of 5 to 100 mg L-1 (Figure 9S, supplementary material). For the quantification of phenanthrene in the sample, the characteristic peak detected at approximately 17.5 min, representing the analyte’s retention time, was used. From the chromatographic data (Figure 10S, supplementary material), the recovery of phenanthrene after the pre-concentration process by SPE was 59%. The evaluation of removing phenanthrene from the aqueous leachate through spectrofluorimetry demonstrated complete removal (100%) from the solution, indicating that the SPE column, supported by the poly(DVB), retained all the contaminant.
4. Conclusions The preliminary batch adsorption tests allowed the individual evaluation of the phenanthrene removal efficiency in aqueous media by ten polymer samples with different monomeric compositions and morphological properties. The polymers containing the Sty monomer or crosslinked with DVB achieved the highest phenanthrene removal efficiency (R = 99.9‒70.3%). We observed that introducing polar monomers into the polymeric structure did not favor the sorption of phenanthrene. The high phenanthrene sorption capacity of poly(DVB) and poly(Sty-co-DVB) was attributed to their large surface area and pore volume as well as the similarity between the Hansen solubility parameters of the monomers and the analyte. The pseudo-second-order model best represented the experimental data for the adsorption kinetics of the two systems studied. Among the diffusion models, the one that best fitted the data was the Urano-Tachikawa model. The column adsorption tests (continuous flow) for phenanthrene removal by poly(DVB) allowed obtaining the saturation point to be obtained by plotting the breakthrough Polímeros, 36(2), e20260022, 2026
curve for the system. Saturation occurred after the elution of approximately 11.8 L of phenanthrene solution (1.0 mg L-1). These studies proved that crosslinked polymers are highly efficient in removing these contaminants from aqueous media. The use of poly(DVB) attained complete removal of phenanthrene (100%) from the aqueous leachate of drill cuttings, indicating that this contaminant was retained by the SPE column containing by this polymer.
5. Author’s Contribution • Conceptualization – Mônica Regina da Costa Marques Calderari; Luciana da Cunha Costa. • Data curation – NA. • Formal analysis – Rafael de Lima Pinto. • Funding acquisition - Mônica Regina da Costa Marques Calderari; Luciana da Cunha Costa. • Investigation – Rafael de Lima Pinto; Ezaine Cristina Corrêa Torquato; Caroline Felix Carvalho. • Methodology – Rafael de Lima Pinto; Ezaine Cristina Corrêa Torquato; Caroline Felix Carvalho. • Project administration – Mônica Regina da Costa Marques Calderari; Luciana da Cunha Costa. • Resources – Mônica Regina da Costa Marques Calderari; Luciana da Cunha Costa. • Software – NA. • Supervision – Mônica Regina da Costa Marques Calderari. • Validation – NA. • Visualization – NA. • Writing – original draft – Rafael de Lima Pinto; Luciana da Cunha Costa. • Writing – review & editing – Luciana da Cunha Costa.
6. Acknowledgements Financing was provided by Coordenação de Aperfeiçoamento de Pessoal de Nível Superior (CAPES), Conselho Nacional de Desenvolvimento Científico e Tecnológico (CNPq), Fundação de Amparo à Pesquisa do Estado do Rio de Janeiro (FAPERJ) and Nitriflex.
7. References 1. Jesus, F., Pereira, J. L., Campos, I., Santos, M., Ré, A., Keizer, J., Nogueira, A., Gonçalves, F. J. M., Abrantes, N., & Serpa, D. (2022). A review on polycyclic aromatic hydrocarbons distribution in freshwater ecosystems and their toxicity to benthic fauna. The Science of the Total Environment, 820, 153282. https://doi. org/10.1016/j.scitotenv.2022.153282. PMid:35066033. 2. Soares, A. S. F., Marques, M. R. C., & Costa, L. C. (2023). Physical chemical characterization and leaching studies involving drill cuttings generated in oil and gas pre salt drilling activities. Environmental Science and Pollution Research International, 30(7), 17899-17914. https://doi.org/10.1007/ s11356-022-23398-7. PMid:36205869. 3. Kravos, A., & Prosen, H. (2024). Exploration of novel solidphase extraction modes for analysis of multiclass emerging contaminants. Analytica Chimica Acta, 1319, 342955. https://doi.org/10.1016/j.aca.2024.342955. PMid:39122271. 7/9
Pinto, R. L., Torquato, E. C. C., Costa, L. C., Carvalho, C. F., & Calderari, M. R. C. M. 4. Ali, A., Qin, T., Zhang, W., Zhang, S., He, L., & Zhao, W. (2025). Recent advances in synthesis and applications of hyper-crosslinked porous organic polymers for sample pretreatment: A review. Analytica Chimica Acta, 1355, 343934. https://doi.org/10.1016/j.aca.2025.343934. PMid:40274337. 5. Maksin, D. D., Nastasović, A. B., Milutinović-Nikolić, A. D., Suručić, L. T., Sandić, Z. P., Hercigonja, R. V., & Onjia, A. E. (2012). Equilibrium and kinetics study on hexavalent chromium adsorption onto diethylene triamine grafted glycidyl methacrylate based copolymers. Journal of Hazardous Materials, 209-210, 99-110. https://doi.org/10.1016/j.jhazmat.2011.12.079. PMid:22284173. 6. Silva, C. M., Rocha, Q. C., Rocha, P. C. S., Louvisse, A. M. T., & Lucas, E. F. (2015). Removal of naphthalene from aqueous systems by poly (divinylbenzene) and poly (methyl methacrylatedivinylbenzene) resins. Journal of Environmental Management, 157, 205-212. https://doi.org/10.1016/j.jenvman.2015.04.025. PMid:25910974. 7. Chen, L., Huang, J., Shi, Y., Peng, X., Kuang, Y., Zhou, S., Zheng, J., Yang, X., & Ouyang, G. (2022). Polystyrene-based nanospheres with controllable microstructures for exceptional solid phase microextraction of organic pollutants. Chemical Engineering Journal, 428, 132527. https://doi.org/10.1016/j. cej.2021.132527. 8. Xu, Q.-N., Wang, H.-L., Zhou, X.-F., Liang, J.-P., Yuan, H., Xu, Y., & Yang, D.-Z. (2022). Micro-mesoporous polystyrene resins prepared by nanosecond pulsed discharge plasma for the efficient adsorption of PAHs. Separation and Purification Technology, 301, 121829. https://doi.org/10.1016/j.seppur.2022.121829. 9. Torquato, E. C. C., Santos, M. M., Cipolatti, E. P., Manoel, E. A., Iulianelli, G. C. V., Pinto, M. C. C., Pinto, R. L., Marques, M. R. C., Pinto, J. C., Guimarães, D. M. F., & Costa, L. C. (2025). Development of biocatalysts based on candida antarctica b lipase immobilized onto crosslinked porous polymers containing varied monomeric compositions. Journal of Applied Polymer Science, 142(19), e56845. https://doi.org/10.1002/app.56845. 10. Association of Official Analytical Chemists - AOAC, & Instituto Nacional de Metrologia, Qualidade e Tecnologia - INMETRO. (2018). Guidance on validation of analytical methods (DOQ-CGCRE-00). Rockville, Maryland: AOAC. 11. Dotto, G. L., Vieira, M. L. G., Gonçalves, J. O., & Pinto, L. A. A. (2011). Removal of acid blue 9, food yellow 3 and fd&c yellow n° 5 dyes from aqueous solutions using activated carbon, activated earth, diatomaceous earth, chitin and chitosan: equilibrium studies and thermodynamic. Química Nova, 34(7), 1193-1199. https://doi.org/10.1590/S0100-40422011000700017.
8/9
12. Evaristo, A. A. A., Santos, K. C. R., Costa, L. C., & Marques, M. R. (2013). Evaluation of ion exchange resins for recovery of metals from electroplating sludge. Polymer Bulletin, 70(8), 2239-2255. https://doi.org/10.1007/s00289-013-0944-x. 13. Fujiwara, N., Nishida, T., & Yamamoto, H. (2019). Adaptation of Hansen solubility parameter in evaluating transparency of composite materials. Heliyon, 5(12), e02833. https://doi. org/10.1016/j.heliyon.2019.e02833. PMid:32083197. 14. Bielicka-Daszkiewicz, K., Voelkel, A., Pietrzyńska, M., & Héberger, K. (2010). Role of Hansen solubility parameters in solid phase extraction. Journal of Chromatography. A, 1217(35), 5564-5570. https://doi.org/10.1016/j.chroma.2010.06.066. PMid:20643412. 15. Lin, X., Jiang, G., & Wang, Y. (2017). Hansen solubility parameters of coal tar-derived typical PAHs using turbidimetric titration and an extended Hansen approach. Journal of Chemical & Engineering Data, 62(3), 954-960. https://doi.org/10.1021/ acs.jced.6b00740. 16. Qin, S.-B., Li, X.-S., Fan, Y.-H., Mou, X.-X., & Qi, S.-H. (2020). Facile synthesis of polydivinylbenzene coated magnetic polydopamine coupled with pressurized liquid extraction for the extraction and cleanup of polycyclic aromatic hydrocarbons in soils. Journal of Chromatography. A, 1613, 460676. https:// doi.org/10.1016/j.chroma.2019.460676. PMid:31727351. 17. Crini, G., Peindy, H. N., Gimbert, F., & Robert, C. (2007). Removal of CI Basic Green 4 (Malachite Green) from aqueous solutions by adsorption using cyclodextrin-based adsorbent: kinetic and equilibrium studies. Separation and Purification Technology, 53(1), 97-110. https://doi.org/10.1016/j.seppur.2006.06.018. 18. Vareda, J. P. (2023). On validity, physical meaning, mechanism insights and regression of adsorption kinetic models. Journal of Molecular Liquids, 376, 121416. https://doi.org/10.1016/j. molliq.2023.121416. 19. Ho, Y.-S. (2006). Review of second-order models for adsorption systems. Journal of Hazardous Materials, 136(3), 681-689. https://doi.org/10.1016/j.jhazmat.2005.12.043. PMid:16460877. 20. Jansson-Charrier, M., Guibal, E., Roussy, J., Delanghe, B., & Le Cloirec, P. (1996). Vanadium (IV) sorption by chitosan: kinetics and equilibrium. Water Research, 30(2), 465-475. https://doi.org/10.1016/0043-1354(95)00154-9. Received: Jul. 05, 2025 Revised: Oct. 13, 2025 Accepted: Feb. 27, 2026 Associate Editor: César L. Petzhold
Polímeros, 36(2), e20260022, 2026
Sorption of phenanthrene by crosslinked polymers with varied monomeric compositions
Supplementary Material Supplementary material accompanies this paper. Table 1S. Data on contact angles and swelling degree in water and methanol of the polymers based on DVB[9]. Table 2S. Data on contact angles and swelling degree in water and methanol of the polymers based on EGDMA[9]. Table 3S. Spectrofluorimetric analysis conditions used in this work to obtain the phenanthrene emission spectra. Table 4S. Equations used to describe phenanthrene sorption efficiency, adsorption capacity, adsorption work capacity, CW (g cm-3). Table 5S. Equations of the kinetic and equilibrium isotherms models used in the experiments[11,12]. Table 6S. Hansen solubility parameters for the monomers used on synthesis of polymeric microspheres (adapted from Torquato et al.)[9]. Table 7S. Hansen solubility parameters for phenanthrene (adapted from Lin et al.)[15]. Table 8S. Sorption capacity data as a function of time (qt) for poly(DVB) and poly(Sty-co-DVB). Figure 1S. (a) Equipment for adsorption experiment in a fixed-bed column; (b) Column packed with polymer used in the experiment. Figure 2S. (a) Superposition of emission spectra of PHE solutions in water; (b) Analytical curve of phenanthrene. Figure 3S. Optical microscopies of DVB-based polymers. (a) poly(DVB); (b) poly(VBC-co-DVB); (c) poly(GMA-co-DVB); (d) poly(MAA-co-DVB); (e) poly(Sty-co-DVB). Figure 4S. Optical microscopies of EGDMA -based polymers. (a) poly(EGDMA); (b) poly(VBC-co-EGDMA); (c) poly(GMA-co-EGDMA); (d) Poly(MAA-co-EGDMA); (e) poly(Sty-co-EGDMA). Figure 5S. Linearization of isotherm models for phenanthrene adsorption on poly(DVB) and poly(Sty-co-DVB) at a temperature of 25 °C: (a) Langmuir; (b) Freundlich. Figure 6S. Linearization of reaction kinetic models for phenanthrene adsorption on poly(DVB) and poli(Sty-co-DVB) at a concentration of 1.0 mg L‒1 and temperature of 25 °C: (a) Pseudo-first order; (b) Pseudo-second order; (c) Elovich. Figure 7S. Linearization of kinetic diffusional models for adsorption of phenanthrene on poly(DVB) and poli(Sty-co-DVB) at a concentration of 1.0 mg L‒1 and temperature of 25 °C: (a) External diffusion; (b) Intraparticle diffusion (Weber-Morris); (c) Intraparticle diffusion (Urano-Tachikawa). Figure 8S. Breakthrough curve of the phenanthrene adsorption process by the poly(DVB). Figure 9S. Calibration curve of phenanthrene by GC-FID. Figure 10S. Chromatogram of: (a) 25 mg L-1 phenanthrene standard; (b) Phenanthrene recovered from drill cuttings leachate by GC-FID. This material is available as part of the online article from https://doi.org/10.1590/0104-1428.0250045
Polímeros, 36(2), e20260022, 2026
9/9
ISSN 1678-5169 (Online)
https://doi.org/10.1590/0104-1428.20250073
Polylactic acid with oat oil: a biodegradable material intended for food packaging Lucas Nunes Fonseca Boechat1 , Rodrigo Gomes de Amorim1 , Fábio Silveira Reis1 , Marianna de Oliveira da Costa Maia Pinto1 , Everton Rangel Bispo2 , Antonieta Middea3 , Edla Maria Bezerra Lima4 , Antonio Renato Bigansolli1 , Danieli Martins do Carmo1 , Belmira Benedita Lima-Kühn1 , Cristiane Hess de Azevedo Meleiro5 , Rosane Nora Castro6 and Renata Nunes Oliveira1* Departamento de Engenharia Química, Universidade Federal Rural do Rio de Janeiro – UFRRJ, Seropédica, RJ, Brasil 2 Centro Universitário Augusto Motta, Rio de Janeiro, RJ, Brasil 3 Centro de Tecnologia Mineral – CETEM, Rio de Janeiro, RJ, Brasil 4 Embrapa Agroindústria de Alimentos, Rio de Janeiro, RJ, Brasil 5 Departamento de Engenharia de Alimentos, Universidade Federal Rural do Rio de Janeiro - UFRRJ, Seropédica, RJ, Brasil 6 Instituto de Química, Universidade Federal Rural do Rio de Janeiro – UFRRJ, Seropédica, RJ, Brasil 1
*renatanunes.ufrrj@gmail.com
Abstract Biodegradable food packaging comprises plastic materials that decompose in the appropriate environment (e.g., moisture and temperature). It could represent a solution for micro- and macroplastic generation. This paper is the first to evaluate the addition of oat oil (OO) to PLA for use as a food packaging material. Samples were evaluated by FTIR, SEM, XRD, Raman, texture and degradation tests. The PLA crystallites and the porosity of the samples increased with increasing oat oil content, while strength decreased (0.14MPa). Regarding degradation, oat oil in the samples facilitated it. Samples with the same composition degraded more in soil (15 weeks) than in seawater (25 weeks). After degradation, the PLA-OO samples were porous, facilitating the entry of fluids and the adhesion of microorganisms. PLA matrix degradation in soil begins with hydrolysis, followed by aerobic microorganisms’ degradation. The highest biodegradation occurred in the PLA-1500 sample in soil, suggesting the potential to achieve biodegradability/compostability. Keywords: biodegradable material, food packaging, oat oil, PLA. Data Availability: All data supporting the findings of this study are available from the corresponding author upon request. How to cite: Boechat, L. N. F., Amorim, R. G., Reis, F. S., Pinto, M. O. C. M., Bispo, E. R., Middea, A., Lima, E. M. B., Bigansolli, A. R., Carmo, D. M., Lima-Kühn, B. B., Azevedo Meleiro, C. H., Castro, R. N., & Oliveira, R. N. (2026). Polylactic acid with oat oil: A biodegradable material intended for food packaging. Polímeros: Ciência e Tecnologia, 36(2), e20260023. https://doi.org/10.1590/0104-1428.20250073
1. Introduction In 2019, plastic packaging was responsible for 142 million tons of plastic waste. It represented 40% of all plastic waste worldwide that year. Among the countries with the highest disposal of plastic packaging in 2019 were China (29.6 Mt) and the USA (26.9 Mt)[1]. In the EU in 2022, 41% of plastic packaging waste was recycled[2]. Brazil ranks 8th in plastic pollution, disposing of 1.3 million tons of plastic in the oceans annually (mostly packaging)[3]. Microplastic pollution currently covers oceans (up to 5.25 trillion microplastics accumulated in the marine environment by 2023[4]), land (an estimated 300 million tonnes accumulated by 2023[5]), and the atmosphere. All living organisms are exposed to microplastics, and their consequences to human health are vast (from neurotoxicity to organ dysfunction)[6].
Polímeros, 36(2), e20260023, 2026
A possible solution to reduce microplastic generation and improper disposal of macroplastics in the oceans would be to replace traditional food packaging with biodegradable alternatives. PLA is a potential biodegradable material for this application. PLA is an aliphatic polyester based on lactic acid monomers. It is considered a biodegradable bioplastic (due to its vegetable origin). However, when discarded, it can persist in the environment for up to 2 years before fully degrading[7]. Nonetheless, PLA is responsible for the formation of non-permanent microplastics, as its degradation kinetics vary with environmental conditions. The ideal degradation conditions would be in controlled composting[8]. PLA can be fully degraded in composting in 6 weeks.
1/11
O O O O O O O O O O O O O O O O
Boechat, L. N. F., Amorim, R. G., Reis, F. S., Pinto, M. O. C. M., Bispo, E. R., Middea, A., Lima, E. M. B., Bigansolli, A. R., Carmo, D. M., Lima-Kühn, B. B., Azevedo Meleiro, C. H., Castro, R. N., & Oliveira, R. N. The marine environment would be among the least conducive to PLA degradation due to the lack of microorganisms involved in this process[9]. It takes approximately 14 months to degrade in a marine environment[10]. PLA-thermoplastic starch (TPS) loaded with epoxidized sesame oil (EPO) intended for food packaging exhibited higher elasticity while maintaining resistance to hydrolytic degradation. TPS was added to PLA to improve adhesion between components and to plasticize the films, while EPO rendered the samples’ surfaces smoother[11]. PLA loaded with epoxidized soy oil (ESO) for sustainable food packaging showed high toughness but delayed degradation. ESO served as a biodegradable plasticizer for PLA[12]. PLA-peppermint oil (PO) samples were suitable for use as antimicrobial materials in prolonged shelf-life food packaging (they were tested with chicken breast). PO granted the antimicrobial properties of these materials[13]. Oat oil is an antioxidant oil with potential for use in active food packaging materials. Among its antioxidants are phenolic compounds, such as avenanthramides (phenolic alkaloids), phenolic acids, e.g., ferulic acid, and flavonoids, e.g., quercetin[14]. Oat grains have high amounts of E-vitamers, where their oils might have lipophilic phytochemicals with tocol groups[15]. Oat oil is used in food preparations[16], and it is not environmentally hazardous[17]. For biodegradable food packaging, it can be a positive additive. PLA is a well-known biodegradable material, and the properties of oat oil may enhance its biodegradation. However, no papers on PLA-oat oil materials for biodegradable food packaging were found in the CAPES database (language: English, simple search, date of search: August 1, 2025, keywords: PLA AND oat oil AND food packaging). The goal of this work is to produce and characterize the properties of PLA-oat oil materials. The samples were characterized using FTIR, Raman spectroscopy, XRD, SEM, and a texture analyser. The samples’ degradation was assessed by weight loss. The Results were organized in two blocks: ‘original samples’ and ‘degraded samples’. In both cases, the Results were presented in the following order (from micro to macro): FTIR, Raman, XRD, SEM, and texture analyser.
2. Materials and Methods Polylactic acid (18 g, 3DLab®) was mixed with 36 mL of dichloromethane at 50 °C under magnetic stirring for 2 h. The solution was then stirred magnetically until it reached room temperature. Oat oil (5-15 ml, Avena sativa L. – Poaceae vegetal oil (100% pure oat oil, Acácia Farmácia de Manipulação®, São Paulo, Brazil)) was added under stirring, and the solution was mixed for 15 minutes. 18 ml of solution was poured onto Petri dishes (Ø 90 mm), covered with tin foil with small holes (needle-size), and dried at room temperature (~30 ºC) for 24 h. The obtained membranes were physiochemically evaluated by FTIR and Raman spectroscopy (kindly executed in CAM/UFRRJ). The FTIR analysis was performed using the equipment FTIR Vertex 70 (Bruker®), with a range of −1 4000 − 500 cm −1, 16 scans per sample, resolution of 4 cm . The Raman spectroscopic analysis used the FT-Raman MultiRAM (Bruker®) software: Opus version 6.5, range of 4000 − 0 cm−1 , LN-Diode Ge detector, Laser Klastech (1064 nm). resolution of 4 cm−1 . 2/11
For the microstructural analysis, the equipment BrukerAXS D8 Advance Eco was used, operating at a tube voltage of 40 kV and Cu kα radiation. The diffractograms were recorded between 2θ = 5 ° to 70 °, 0.02 ° step, and a positionsensitive LynxEye detector (Karlsruhe, Germany). The morphological analysis was performed using a Hitachi TM3030Plus (Tokyo, Japan) scanning electron microscope (SEM) at 15 kV, with an integrated EDS (Bruker Quantax 70, Karlsruhe, Germany). Both analyses were kindly performed at CETEM. Texture analysis was used to evaluate the mechanical properties of the samples before and after degradation (samples were placed in soil for 3 months and hydrated, following a similar degradation pattern in the soil degradation method). Triplicates (samples of Ø 90mm, thickness of ~0.7mm) were used. The probe used in the texture analysis (Stable Micro Systems, TA.XT Plus) had a diameter of 5 mm. The degradation analysis was performed in soil (humus from Rio de Janeiro, Brazil) and seawater, with seawater pH measured weekly, using universal pH paper (Kasvi®). For the soil degradation test, at least nine samples of each composition were used (an area of approximately 1 cm2, thickness of ~0.7 cm). The samples were weighed and buried in 35g of soil (in the middle of the container). Once a week, the soil was hydrated with 5ml of water. The containers were kept open, and the samples were washed and dried (superficially with tissue paper to remove adsorbed water) weekly to measure their weight. By the end of the test (intended to last 6 months), each container’s contents were placed in a 2 mm opening sieve and wet-sieved with a constant water flow. The retained material was weighed and dried in an oven (50ºC, 24h), a methodology adapted from ABNT NBR 15448-2 standard. For the seawater degradation test, 20 mL of seawater was placed in individual containers. At least nine samples of each composition were used. The samples were weighed and placed inside seawater. The pH of the water and the samples’ weight were measured weekly. Software OriginPro® was used for ANOVA and the Tukey test (95% confidence level). The samples’ degradation in seawater and soil was evaluated statistically using a 2-way ANOVA and a Tukey test (factors: composition (4 levels: PLA, PLA-5OO, PLA-10OO, and PLA-15OO) and media (2 levels: seawater and soil)), with a 95% confidence level for both.
3. Results and Discussions 3.1 Original (non-degraded) samples The results for FTIR, Raman, XRD, and texture analysis of the non-degraded (original) samples were grouped in the Supplementary file (Figure S1, Table S1, and Table S2), while their SEM images were displayed in Figure 1. 3.1.1 FTIR The main FTIR bands of all samples can be related to PLA. There was an oat oil band at 1159 cm−1 ( ν ( C − O ) of aliphatic esters or δ ( CH 2 ) vibrations)[18]. As the amount of oat oil in the samples increases, the small shoulder at 1199 cm−1 in PLA sample turns into a small band. Polímeros, 36(2), e20260023, 2026
Polylactic acid with oat oil: a biodegradable material intended for food packaging
Figure 1. SEM images of original samples (non-degraded): (a) PLA, (b) PLA-5OO, (c) PLA-10OO, (d) PLA-15OO.
This slight change might be the overlap of the oat oil band at 1157 cm−1 with the small shoulder of PLA at 1199 cm−1 . No evidence of chemical bonding (FTIR bands’ absence, FTIR bands’ shift, or new FTIR bands not related to PLA or oat oil) was observed[19]. 3.1.2 Raman PLA’s Raman spectrum presented its prominent characteristic peaks. Oat oil usually presents fatty acids (mainly palmitic, oleic, linoleic, and stearic acids)[20]. Most oat oil bands were identified only in samples with high amounts of these oils (PLA-10OO and PLA-15OO). No chemical or physical interactions were observed. 3.1.3 XRD PLA samples presented the following XRD characteristic peaks (decrescent intensity): 2θ = 16.4º , PLA crystallographic plans ( 200 ) / (110 ) of α − form crystals; 2θ = 18.7º , crystallographic plan ( 203) ; 2θ = 22.1º , crystallographic plan ( 015) [21]; 2θ = 28.8º , crystallographic plan ( 216 ) [22]. The addition of oat oil increased the PLA diffraction peaks intensity, besides revealing several other PLA low intensity peaks: 2θ = 12.2º , crystallographic plan (103)[23]; 2θ = 14.5º , crystallographic plan ( 010 ) [21]; 2θ = 31.1º , which is considered indicative of PLA amorphous phase[24]. The crystal size of PLA’s α − crystals increased as the amount of oat oil was higher in the samples, which might be related to weak interaction or even phase separation Polímeros, 36(2), e20260023, 2026
between PLA and oat oil[25]. Phase separation could initially create regions rich in PLA, increasing contact between PLA chains and increasing the size of PLA crystals[26]. 3.1.4 SEM SEM analysis of the original (non-degraded) samples (Figure 1) revealed that increasing the amount of oil in the samples increased the pore diameter[27]. The oat oil seems to turn the samples into a sponge-like material. The oat oil was probably dispersed in PLA as micrometric droplets, whose size increased with the amount of oil in the samples. Part of the PLA chains were packed together between oat oil droplets, stimulating chain organization (increasing the size of PLA crystallites, as indicated by XRD). 3.1.5 Texture analysis The addition of oat oil diminishes the samples’ strength
( )
p = 3.34 10−8 (Supplementary file, Figure S1). Tukey test
revealed that samples with a high amount of oil (PLA-15OO) are weaker than the other samples ( p < 4.62 10−4 ) . The oat oil acted as a plasticizer, so it would remain between PLA’s amorphous chains, facilitating their movement under mechanical stress[28]. The amount of oat oil in the samples is enough to act as a plasticizer (in amorphous PLA), while its excess would be dispersed in PLA as microdroplets (due to partial affinity between PLA and oat oil[29]), as indicated by XRD and SEM.
( )
3/11
Boechat, L. N. F., Amorim, R. G., Reis, F. S., Pinto, M. O. C. M., Bispo, E. R., Middea, A., Lima, E. M. B., Bigansolli, A. R., Carmo, D. M., Lima-Kühn, B. B., Azevedo Meleiro, C. H., Castro, R. N., & Oliveira, R. N. 3.2 Degraded samples Degradation results were the first ones presented, followed by the analysis performed on the degraded samples: FTIR, Raman, texture, SEM, XRD. 3.2.1 Degradation tests The samples’ seawater degradation continued for 25 weeks, after which the samples broke into small pieces (< 2 mm). The test was interrupted. The same evaluation (samples were considered biodegraded when they broke into pieces smaller than 2 mm) was applied to samples buried in soil, but 15 weeks were sufficient for them to be considered biodegraded (Supplementary file, Figure S2). There was a significant difference in degradation between compositions, with samples containing more oat oil degrading more, p = 2.65 10−4 . In addition, the Tukey test indicated
( )
of the spectrum after soil immersion, sign of samples’ degradation[41]. There was also a shift in some bands (from [42] 1043 to1031cm −1 ( ν s ( C − O − C ) ) and from 919 to 910 cm −1 ( C − C backbone vibration and ρ ( CH3 ) of PLLA α crystals[43])), also indicating degradation[44]. In addition, there are indications of PLA degradation, as well as soil/ clay adsorption, throughout the bands at 3697 cm−1 ( −OH vibration, where the formation of carboxylic acid justifies the presence of this band. The breakage of the PLA chains rises the number of carboxylic chains’ ends[45]); 3621cm−1 (probably due to complex structural OH of clays present in soil/humus[46]); 1002 cm−1 (quartz’ ν ( Si − O ) and ν ( Si − O − Si ) groups in soil[47]); more intense band at 912 cm−1 (kaolinite’s ( O − Al − OH ) vibration); 532 and 466 cm−1 , related to soil ( δ ( Si − O − Al ) and δ in plane ( Si − O − Si ) , respectively[37]); and 410 cm −1 (quartz’ δ ( O − Si − O )
).
[48]
that samples with the same composition degraded more in soil than in seawater. PLA samples are usually more resistant to seawater degradation than soil. This behaviour could be due to a lack of biofilm formation/maintenance in seawater[10]. All samples were smaller than 2 mm and were considered degraded. However, it took more than 12 weeks to fully biodegrade in soil, so they cannot be regarded as compostable under the Brazilian standard[30].
The PLA-10OO sample, after immersion in seawater, also presented the band at 1537 cm−1 , related to the cellulose in seawater[40]. The PLA-10OO sample buried in the soil also degraded and adsorbed soil, showing bands similar to those of the PLA-5OO buried samples. The PLA-10OO buried sample also presented bands at: 1585 cm−1 (remaining biofilm of anaerobic degradation[49]), revealing even more details of these samples’ degradation; 428 cm−1 soil’s clays ( δ ( Si − O − Mg ) [50]).
3.2.2 FTIR
After seawater, the sample PLA-15OO presented an extra band at 1405 cm−1 , probably δ as ( CH 3 ) [51] vibration, an indication of the samples’ degradation. After burial in soil, PLA-15OO samples presented the previously described soil bands, as well as PLA chain breakage (hydrolysis and microbial degradation). There is also an extra band at 1502 cm−1 , related to soil’s wood lignin[52] residue adsorbed in the samples; as well as an extra soil’s band at 543 cm−1 ( Si − O − Al )[53]. The PLA band at ~730 cm−1 ( C = O ) [54] is absent.
All curves were normalized to present 100% transmission at 4000 cm-1. All samples were maintained in soil or seawater for several weeks (25 in seawater and 15 in soil), and FTIR revealed changes associated with degradation (Supplementary file, Figure S3). Degraded PLA (in both seawater and soil, since the patterns are similar) presented bands’ absence ( 2923 and 2854 cm−1 , besides the band at 750 cm−1 , where this previous band is currently a shoulder), bands displacement (from 919 to 914 cm−1; from 1081to1085 cm−1 ; from 1263 to1267 cm−1 ) and new bands (at 3004,1201 (it was a shoulder before degradation) 536, and 466 cm −1 ). The absence of the bands at 2923 and 2854 cm−1 indicate PLA disintegration[31], while the decrease of the band’s intensity at 750 cm−1 is related to oxidation[32]. Bands shift could be related to PLA’ chains scissions during the degradation process[33]. The band at 3004 cm−1 indicates the presence of lactide’s ν ( C − H ) vibration[34], a monomeric degradation product of PLA[35]. The band at 1201cm−1 represents ν ( C − O ) vibration of lactide[36]. The bands at 536 and 466 cm−1 can be related to soil ( δ ( Si − O − Al ) and δ in plane ( Si − O − Si ) , respectively[37]) or due to quartz and kaolinite that occur in Brazilian southeast sea[38]. In the PLA-5OO sample, after immersion in seawater, two bands were revealed at 1575 and1540 cm−1 . The first one is related to PLA, the −C = O vibrations of the ketone group (linked to aliphatic polyester and probably to amorphous PLA)[39], while the last band would be related to adsorbed cellulose ( ν ( C= C − C ) of aromatics), or to amides’ δ ( N − H ) andν ( C − N )) present in seawater[40]. There was more altering in PLA-5OO samples degraded in soil compared to seawater. The PLA bands at 958, 750, and 698 cm−1 were not part 4/11
3.2.3 Raman The Raman spectra of PLA before and after degradation in seawater presented the same peaks (Supplementary file, Figure S4), with slight changes in the Raman Intensity. The peaks at 919, 737, and 703cm−1 were more intense after immersion in seawater. Their vibrational modes would be, respectively, ρ ( CH3 ) + ν ( CC ) ; δ ( C = O ) ; and
γ ( C = O ) [55]. The increase of ρ ( CH3 ) + ν ( CC ) would be due to conformational changes during degradation[56]. The observation of PLA degradation in an aqueous environment (as evidenced by FTIR and degradation analysis) often results in the formation of free C=O groups, which yield a more intense signal[57]. After immersion in seawater, besides the PLA and OO characteristic peaks, PLA-10OO and PLA-15OO samples presented a peak at 1652 cm−1, which can be attributed to residual moisture or C = C groups (a consequence of the polymer degradation)[58]. After burial in soil, all the samples presented the absence of the following bands: 1749,1370,1292,1212, 1178, 919, 735, and 707 cm−1. Degradation is usually responsible for the absence of some peaks after immersion in the media[59]. In the present analysis, it was observed for the samples immersed in soil (as corroborated by FTIR and degradation tests).
Polímeros, 36(2), e20260023, 2026
Polylactic acid with oat oil: a biodegradable material intended for food packaging 3.2.4 XRD The intensity of PLA’s XRD peaks varied after degradation (Supplementary file, Figure S5). After seawater degradation, PLA’s crystal peaks are more intense, indicating chain scission in the amorphous regions[60]. The rise of some PLA crystallites’ size after degradation and the diminishment of the amorphous halo could result from secondary crystallization (initiated during the hydrolysis of amorphous PLA)[61]. The diminution of other crystallite sizes indicates further degradation: after the secondary crystallization, the polymeric chains are shortened[62]. Degradation in soil and seawater differs because soil contains microorganisms (fungi and bacteria). These organisms produce several enzymes that adhere to the PLA samples and
accelerate the biodegradation[63]. The highest degradation occurred in the PLA-15OO sample in soil. However, all soil-degrading samples can be considered in a subsequent degradation step, as previously indicated (FTIR, Raman, and degradation tests). 3.2.5 SEM Samples degraded in seawater showed salt crystals on their surfaces (Figures 2 and 3), but they were observed only in samples PLA-10OO and PLA-15OO. EDX quantified sea salt (NaCl) deposition on samples PLA-15OO degraded in seawater. Besides carbon and oxygen, the main elements found in these samples were sodium and chlorine. In addition, irregular/bumpy particles form on the sample surface[64].
Figure 2. SEM images of samples degraded in seawater on the samples’ surface: (a) PLA, (b) PLA-5OO, (c) PLA-10OO, (d) PLA-15OO with salt crystals spread over the samples’ surfaces, (e) EDX of the sample PLA-15OO degraded in seawater and (f) Na EDX map, (g) Elements ID by EDX. Polímeros, 36(2), e20260023, 2026
5/11
Boechat, L. N. F., Amorim, R. G., Reis, F. S., Pinto, M. O. C. M., Bispo, E. R., Middea, A., Lima, E. M. B., Bigansolli, A. R., Carmo, D. M., Lima-Kühn, B. B., Azevedo Meleiro, C. H., Castro, R. N., & Oliveira, R. N.
Figure 3. SEM images of samples degraded in soil: (a) PLA, (b) PLA-5OO, (c) PLA-10OO, (d) PLA-15OO. White arrows indicate filamentous microorganisms adhered to the surface of the samples PLA-10OO and PLA-15OO; (e) EDX of PLA-15OO sample degraded in soil, and (f) Si EDX map, (g) Elements ID by EDX.
Samples’ delayed degradation in seawater can be attributed to seawater’s higher surface tension than that of distilled water, which makes it more difficult for seawater to enter the samples’ pores for hydrolysis[57]. The PLA sample porosity after seawater immersion could reveal sample degradation compared to the non-degraded PLA sample (hydrolytic degradation, as indicated by FTIR, Raman, and degradation tests). Sample degradation was high in the soil (hydrated weekly), as indicated by FTIR. In PLA samples, which were originally non-porous, holes were observed on the surface (blocked by soil filling). These channels were used by water and microorganisms for degradation. The PLA-OO samples were initially porous, facilitating the entry of fluids and the adhesion of microorganisms. PLA degradation in 6/11
soil usually begins with hydrolysis, followed by aerobic microbial degradation[65]. The EDX showed that, besides the polymer elements (C, O, and H), Si, Al, Ti, and Fe were the main elements found in samples PLA-15OO degraded in soil, probably in the soil’s clays[66]. The presence of adhered filamentous microorganisms was identified, which could be soil’s fungal hyphae[67]. Samples’ rapid degradation in soil is attributed to the presence of PLA and oat oil, which are readily available to microorganisms. 3.2.6 Texture analysis Sample degradation in soil was superior to that in seawater. To evaluate the impact of biodegradation on the samples’ mechanical strength, texture analysis was performed after 12 weeks of soil immersion (Supplementary file, Figure S6). Polímeros, 36(2), e20260023, 2026
Polylactic acid with oat oil: a biodegradable material intended for food packaging Biodegradation in soil diminishes the samples’ strength p = 1.19 10−5 . In addition, biodegraded samples with high
( )
amounts of oat oil (PLA-10OO and PLA-15OO) presented lower strength than the other biodegraded samples (p < 0.03). The biodegraded PLA-10OO and PLA-15OO were also weaker than all the original (non-degraded) samples ( p < 2.21 10−5 ). When thermos-oxidative degradation occurs, as chain size diminishes, the samples become brittle, and their strength decreases considerably[32]. Usually, the decrease in strength due to biodegradation is correlated with PLA hydrolysis[68].
( )
4. Conclusions PLA-OO samples presented all characteristic FTIR and Raman bands/peaks of PLA and oat oil’s fatty acids. The PLA crystallite size and sample porosity increased with increasing oat oil content, indicative of phase separation. In contrast, adding oil resulted in a plasticizer effect on the mechanical properties. It is indicative of partial affinity. Regarding degradation, oat oil in the samples accelerated it and significantly reduced the samples’ strength. Samples with the same composition degraded more in soil than in seawater. After immersion in soil and seawater, sample degradation was observed by the absence of bands in the FTIR spectrum, and adsorbed material (cellulose, clays, microorganisms) was identified, along with unexpected FTIR bands. Raman identified that PLA-OO samples degraded hydrolytically in seawater and soil, a key step in PLA degradation. However, sample degradation in seawater is delayed by seawater’s high surface tension, which makes it difficult for hydrolysis to enter the sample’s pores. The samples with high amounts of oil (PLA-10OO and PLA15OO) that were biodegraded (soil) were weaker than the other biodegraded samples, as well as the original PLA, PLA-5OO, and PLA-10OO ones. The PLA-OO samples were initially more porous than PLA, facilitating fluid entry and microorganism adhesion. PLA matrix degradation in soil begins with hydrolysis, followed by aerobic microbial degradation, which is partially attributed to adhered fungi. Fast degradation in soil is attributed not only to PLA but also to oat oil. All samples immersed in soil can be considered to undergo further degradation than those in seawater. The highest degradation occurred in the PLA-15OO sample in soil. PLA-oat oil materials present the potential to reach biodegradability/compostability.
5. Author’s Contribution • Conceptualization – Renata Nunes Oliveira; Lucas Nunes Fonseca Boechat; Marianna de Oliveira da Costa Maia Pinto; Cristiane Hess de Azevedo Meleiro. • Data curation – Lucas Nunes Fonseca Boechat; Rodrigo Gomes de Amorim; Fábio Silveira Reis. • Formal analysis – Edla Maria Bezerra Lima; Renata Nunes Oliveira. • Funding acquisition - Renata Nunes Oliveira. • Investigation – Lucas Nunes Fonseca Boechat; Rodrigo Gomes de Amorim; Fábio Silveira Reis. Polímeros, 36(2), e20260023, 2026
• Methodology – Antonieta Middea; Edla Maria Bezerra Lima; Lucas Nunes Fonseca Boechat; Rodrigo Gomes de Amorim; Fábio Silveira Reis; Renata Nunes Oliveira. • Project administration – Renata Nunes Oliveira. • Resources – Renata Nunes Oliveira; Antonieta Middea; Edla Maria Bezerra Lima; Rosane Nora Castro. • Software – Renata Nunes Oliveira. • Supervision – Renata Nunes Oliveira. • Validation – Antonio Renato Bigansolli; Danieli Martins do Carmo; Belmira Benedita Lima-Kühn; Renata Nunes Oliveira. • Visualization – Lucas Nunes Fonseca Boechat; Rodrigo Gomes de Amorim; Fábio Silveira Reis; Renata Nunes Oliveira. • Writing – original draft – Renata Nunes Oliveira. • Writing – review & editing – Lucas Nunes Fonseca Boechat; Rodrigo Gomes de Amorim; Fábio Silveira Reis; Marianna de Oliveira da Costa Maia Pinto; Antonieta Middea; Edla Maria Bezerra Lima; Antonio Renato Bigansolli; Danieli Martins do Carmo; Belmira Benedita Lima-Kühn; Cristiane Hess de Azevedo Meleiro; Rosane Nora Castro; Everton Rangel Bispo; Renata Nunes Oliveira.
6. Acknowledgements The authors thank the National Council for Scientific and Technological Development – CNPq, process 406033/2022-6, for the funding grant and the Ministry of Science, Technology and Innovation – MCTI. This study was financed in part by the Coordenação de Aperfeiçoamento de Pessoal de Nível Superior – Brasil (CAPES) – Finance Code 001. The authors also thank CAM/UFRRJ and CETEM for the analysis performed.
7. References 1. Samborska, V. (2019). Packaging is the source of 40% of the planet’s plastic waste. Our World in Data. Retrieved in 2025, August 10, from https://ourworldindata.org/plastic-pollution 2. Eurostat. (2024). 41% of plastic packaging waste recycled in 2022. Retrieved in 2025, August 10, from https://ec.europa. eu/eurostat 3. Sinimbú, F. (2024). Brazil dumps 1.3M tons of plastic into the ocean every year. Agência Brasil. Retrieved in 2025, August 10, from https://agenciabrasil.ebc.com.br/en/meio-ambiente/ noticia/2024-10/brazil-dumps-13m-tons-plastic-ocean-everyyear 4. Ribó, M., Watson, S. J., Novikova, N. I., Deppeler, S., Seabrook, S., Hale, R., & Strachan, L. J. (2023). Microplastic pollution distribution: differences between marine reserves and urbanised areas. Continental Shelf Research, 267, 105115. https://doi. org/10.1016/j.csr.2023.105115. 5. Haque, F., & Fan, C. (2023). Fate and impacts of microplastics in the environment: hydrosphere, pedosphere, and atmosphere. Environment, 10(5), 70. https://doi.org/10.3390/ environments10050070. 6. Li, Y., Tao, L., Wang, Q., Wang, F., Li, G., & Song, M. (2023). Potential health impact of microplastics: a review of environmental distribution, human exposure, and toxic effects. Environment & Health, 1(4), 249-257. https://doi.org/10.1021/ envhealth.3c00052. PMid:39474495. 7/11
Boechat, L. N. F., Amorim, R. G., Reis, F. S., Pinto, M. O. C. M., Bispo, E. R., Middea, A., Lima, E. M. B., Bigansolli, A. R., Carmo, D. M., Lima-Kühn, B. B., Azevedo Meleiro, C. H., Castro, R. N., & Oliveira, R. N. 7. Velghe, I., Buffel, B., Vandeginste, V., Thielemans, W., & Desplentere, F. (2023). Review on the degradation of poly(lactic acid) during melt processing. Polymers, 15(9), 2047. https://doi.org/10.3390/polym15092047. PMid:37177194. 8. Ainali, N. M., Kalaronis, D., Evgenidou, E., Kyzas, G. Z., Bobori, D. C., Kaloyianni, M., Yang, X., Bikiaris, D. N., & Lambropoulou, D. A. (2022). Do poly(lactic acid) microplastics instigate a threat? A perception for their dynamic towards environmental pollution and toxicity. The Science of the Total Environment, 832, 155014. https://doi.org/10.1016/j.scitotenv.2022.155014. PMid:35381252. 9. Ahsan, W. A., Hussain, A., Lin, C., & Nguyen, M. K. (2023). Biodegradation of different types of bioplastics through composting: a recent trend in green recycling. Catalysts, 13(2), 294. https://doi.org/10.3390/catal13020294. 10. Royer, S.-J., Greco, F., Kogler, M., & Deheyn, D. D. (2023). Not so biodegradable: polylactic acid and cellulose/plastic blend textiles lack fast biodegradation in marine waters. PLoS One, 18(5), e0284681. https://doi.org/10.1371/journal. pone.0284681. PMid:37224114. 11. Bohórquez-Ayala, M., Rojano-Quiroz, D., González-Cuello, R., García-Zapateiro, L., & Ortega-Toro, R. (2021). Application of modified vegetable oil for improvement of biodegradable materials based on thermoplastic starch and polylactic acid. Revista Mexicana de Ingeniería Química, 20(1), 423-433. https://doi.org/10.24275/rmiq/Poly2164. 12. Zych, A., Perotto, G., Trojanowska, D., Tedeschi, G., Bertolacci, L., Francini, N., & Athanassiou, A. (2021). Super tough polylactic acid plasticized with epoxidized soybean oil methyl ester for flexible food packaging. ACS Applied Polymer Materials, 3(10), 5087-5095. https://doi.org/10.1021/acsapm.1c00832. 13. Emir, A. A., Yildiz, E., & Kirtil, E. (2024). Peppermint oil‐ infused polylactic acid films: a novel approach for antimicrobial and biodegradable food packaging. Polymer Engineering and Science, 64(6), 2943-2955. https://doi.org/10.1002/pen.26737. 14. Paudel, D., Dhungana, B., Caffe, M., & Krishnan, P. (2021). A review of health-beneficial properties of oats. Foods, 10(11), 2591. https://doi.org/10.3390/foods10112591. PMid:34828872. 15. White, D. A., Fisk, I. D., & Gray, D. A. (2006). Characterisation of oat (Avena sativa L.) oil bodies and intrinsically associated E-vitamers. Journal of Cereal Science, 43(2), 244-249. https://doi.org/10.1016/j.jcs.2005.10.002. 16. Robards, K., Prenzler, P., Ryan, D., & Kamal-Eldin, A. (2009). Oat oil. In R. A. Moreau, & A. Kamal-Eldin (Eds.), Gourmet and health-promoting specialty oils (pp. 433-454). Urbana: AOCS Press. https://doi.org/10.1016/B978-1-893997-97-4.50022-X. 17. Indo Bio Organics. (2025). Oat oil (Material Safety Data Sheet – MSDS 231). Retrieved in 2025, August 10, from https://essentialoilsofindia.com/product/oat-oil/ 18. Zhang, H., Ma, J., Miao, Y., Tuchiya, T., & Chen, J. Y. (2015). Analysis of carbonyl value of frying oil by fourier transform infrared spectroscopy. Journal of Oleo Science, 64(4), 375-380. https://doi.org/10.5650/jos.ess14201. PMid:25766931. 19. Şen, İ., Atagür, M., Tuna, S., Eroğlu, M., Kurtlu, M. A., & Sever, K. (2024). Manufacturing and characterization of three modified vegetable oil-added polylactic acid composites. International Journal of Polymer Science, 2024(1), 3259882. https://doi.org/10.1155/2024/3259882. 20. Banaś, K., & Harasym, J. (2021). Current knowledge of content and composition of oat oil: future perspectives of oat as oil source. Food and Bioprocess Technology, 14(2), 232-247. https://doi.org/10.1007/s11947-020-02535-5. 21. Frone, A. N., Ghiurea, M., Nicolae, C. A., Gabor, A. R., Badila, S., & Panaitescu, D. M. (2022). Poly(lactic acid)/ poly(3-hydroxybutyrate) biocomposites with differently treated cellulose fibers. Molecules, 27(8), 2390. https://doi. org/10.3390/molecules27082390. PMid:35458593. 8/11
22. Puchalski, M., Kwolek, S., Szparaga, G., Chrzanowski, M., & Krucińska, I. (2017). Investigation of the influence of PLA molecular structure on the crystalline forms (α′ and α) and mechanical properties of wet spinning fibres. Polymers, 9(1), 18. https://doi.org/10.3390/polym9010018. PMid:30970693. 23. Farid, T., Herrera, V. N., & Kristiina, O. (2018). Investigation of crystalline structure of plasticized poly (lactic acid)/Banana nanofibers composites. IOP Conference Series. Materials Science and Engineering, 369, 012031. https://doi.org/10.1088/1757899X/369/1/012031. 24. Vozniak, A., & Bartczak, Z. (2021). Deformation of poly-llactid acid (PLLA) under uniaxial tension and plane-strain compression. Polymers, 13(24), 4432. https://doi.org/10.3390/ polym13244432. PMid:34960984. 25. Kale, R. D., & Gorade, V. G. (2018). Preparation of acylated microcrystalline cellulose using olive oil and its reinforcing effect on poly(lactic acid) films for packaging application. Journal of Polymer Research, 25(3), 81. https://doi.org/10.1007/ s10965-018-1470-1. 26. Hu, Y., Hu, Y. S., Topolkaraev, V., Hiltner, A., & Baer, E. (2003). Crystallization and phase separation in blends of high stereoregular poly(lactide) with poly(ethylene glycol). Polymer, 44(19), 5681-5689. https://doi.org/10.1016/S0032-3861(03)00609-8. 27. Munteanu, B. S., & Vasile, C. (2021). Encapsulation of natural bioactive compounds by electrospinning: applications in food storage and safety. Polymers, 13(21), 3771. https://doi. org/10.3390/polym13213771. PMid:34771329. 28. Carpintero, M., Marcet, I., Rendueles, M., & Díaz, M. (2021). Egg yolk oil as a plasticizer for polylactic acid films. Membranes, 12(1), 46. https://doi.org/10.3390/membranes12010046. PMid:35054572. 29. Yusoff, N. H., Pal, K., Narayanan, T., & Souza, F. G. (2021). Recent trends on bioplastics synthesis and characterizations: polylactic acid (PLA) incorporated with tapioca starch for packaging applications. Journal of Molecular Structure, 1232, 129954. https://doi.org/10.1016/j.molstruc.2021.129954. 30. Associação Brasileira de Normas Técnicas – ABNT. (2008). ABNT NBR 15448-2: embalagens plásticas degradáveis e/ou de fontes renováveis. Parte 2: biodegradação e compostagem: requisitos e métodos de ensaio. Rio de Janeiro. Retrieved in 2025, August 10, from https://www.normas.com.br/visualizar/ abnt-nbr-nm/26890/abnt-nbr15448-2-embalagens-plasticasdegradaveis-e-ou-de-fontes-renovaveis-parte-2-biodegradacaoe-compostagem-requisitos-e-metodos-de-ensaio 31. Udayakumar, M., Zsoldos, G., & Kollár, M. (2017). Study on effect of degradation of poly(lactic acid) on its properties. In XXXI MicroCAD International Scientific Conference, Miskolc, Hungary. Miskolc: University of Miskolc. https://doi.org/10.26649/ musci.2017.036. 32. Rasselet, D., Ruellan, A., Guinault, A., Miquelard-Garnier, G., Sollogoub, C., & Fayolle, B. (2014). Oxidative degradation of polylactide (PLA) and its effects on physical and mechanical properties. European Polymer Journal, 50, 109-116. https://doi.org/10.1016/j.eurpolymj.2013.10.011. 33. Leroy, A., Ribeiro, S., Grossiord, C., Alves, A., Vestberg, R. H., Salles, V., Brunon, C., Gritsch, K., Grosgogeat, B., & Bayon, Y. (2017). FTIR microscopy contribution for comprehension of degradation mechanisms in PLA-based implantable medical devices. Journal of Materials Science. Materials in Medicine, 28(6), 87. https://doi.org/10.1007/s10856-017-5894-7. PMid:28470445. 34. Mili, M., Gupta, A., Monika, & Katiyar, V. (2017). Designing of poly(l-lactide)–nicotine conjugates: mechanistic and kinetic studies and thermal release behavior of nicotine. ACS Omega, 2(9), 6131-6142. https://doi.org/10.1021/acsomega.7b01002. PMid:31457860. Polímeros, 36(2), e20260023, 2026
Polylactic acid with oat oil: a biodegradable material intended for food packaging 35. Hussain, M., Khan, S. M., Shafiq, M., & Abbas, N. (2024). A review on PLA-based biodegradable materials for biomedical applications. Giant, 18, 100261. https://doi.org/10.1016/j. giant.2024.100261. 36. Rahmayetty, S., Prasetya, B., & Gozan, M. (2015). Effect of temperature and concentration of SnCl2 on depolymerization process of L-lactide synthesis from l-lactic acid via short polycondensation. International Journal of Applied Engineering Research, 10(21), 41942-41946. Retrieved in 2025, August 10, from https://www.ripublication.com/ ijaer10/ijaerv10n21_42.pdf 37. Islam, M. M., Khan, M. N., Biswas, S., Choudhury, T. R., Haque, P., Rashid, T. U., & Rahman, M. M. (2017). Preparation and characterization of bijoypur clay-crystalline cellulose composite for application as an adsorbent. Advanced Material Science, 2(3), 1-7. https://doi.org/10.15761/AMS.1000126. 38. Carvalho, A. C. B., Silva, L. J., Dick, D. P., Moreira, V. A., Vicente, M. C., Andrade, A. F. O., Bidone, E. D., & SabadiniSantos, E. (2020). Análise espectroscópica da matéria orgânica no sedimento superficial da baía de sepetiba, Rio de Janeiro, Brasil. Química Nova, 43(5), 552-557. https://doi. org/10.21577/0100-4042.20170518. 39. Sriram, M., Kadhirnilavan, R., Mohammed, K. A. N., Kumar, S. A., Mishra, A., & Tiwari, A. (2023). Bio-based PLA membranes for ion transport and ion filtration. Journal of Research Updates in Polymer Science, 12, 220-230. https://doi.org/10.6000/19295995.2023.12.21. 40. Merino, D., Zych, A., & Athanassiou, A. (2022). Biodegradable and biobased mulch films: highly stretchable PLA composites with different industrial vegetable waste. ACS Applied Materials & Interfaces, 14(41), 46920-46931. https://doi.org/10.1021/ acsami.2c10965. PMid:36198101. 41. Xiao, S., Cui, X., & Iroh, J. O. (2023). A study of the degradation mechanism of ladder-like polyhedral oligomeric silsesquioxane via Fourier transform infrared spectroscopy. Fire, 6(11), 429. https://doi.org/10.3390/fire6110429. 42. Savaris, M., Braga, G. L., Santos, V., Carvalho, G. A., Falavigna, A., Machado, D. C., Viezzer, C., & Brandalise, R. N. (2017). Biocompatibility assessment of poly(lactic acid) films after sterilization with ethylene oxide in histological study in vivo with wistar rats and cellular adhesion of fibroblasts in vitro. International Journal of Polymer Science, 2017(1), 7158650. https://doi.org/10.1155/2017/7158650. 43. Farahani, A., Zarei-Hanzaki, A., Abedi, H. R., Tayebi, L., & Mostafavi, E. (2021). Polylactic acid piezo-biopolymers: chemistry, structural evolution, fabrication methods, and tissue engineering applications. Journal of Functional Biomaterials, 12(4), 71. https://doi.org/10.3390/jfb12040071. PMid:34940550. 44. Wilfred, O., Tai, H., Marriott, R., Liu, Q., Tverezovskiy, V., Curling, S., Tai, H., & Fa, Z. (2018). Biodegradation of polylactic acid and starch composites in compost and soil. International Journal of Nano Research, 1(2), 1-11. Retrieved in 2025, August 10, from https://www.innovationinfo.org/ articles/IJNR/IJNR-1-107.pdf 45. Benhami, V. M. L., Longatti, S. M. O., Moreira, F. M. S., & Sena Neto, A. R. (2024). Biodegradation of poly(lactic acid) waste from 3D printing. Polímeros: Ciência e Tecnologia, 34(2), e20240013. https://doi.org/10.1590/0104-1428.20230058. 46. Ahmed, N., Purakaystha, T. J., Das, R., Biswas, S., & Datta, S. C. (2019). Assessment of clay-humus stability through IR spectroscopy in a long-term integrated nutrient management experiment. In Proceedings of the 22nd Annual Convention of the Clay Minerals Society of India and National Conference on Application of Clay and Allied Sciences in Agriculture, Environment and Industry, New Delhi, India. New Delhi: ICAR-IARI. Polímeros, 36(2), e20260023, 2026
47. Ene, A., Moraru, S. S., Moraru, D. I., Pantelica, A., Gosav, S., & Ceoromila, A. M. (2024). Major and trace element accumulation in soils and crops (wheat, corn, sunflower) around steel industry in the lower danube basin and associated ecological and health risks. Applied Sciences, 14(13), 5616. https://doi.org/10.3390/app14135616. 48. Volkov, D. S., Rogova, O. B., & Proskurnin, M. A. (2021). Temperature dependences of IR spectral band frequencies of soils. In Proceedings of the 7th World Congress on New Technologies (NewTech’21). Virtual conference. https://doi. org/10.11159/icepr21.115. 49. Bracciale, M. P., De Gioannis, G., Falzarano, M., Muntoni, A., Polettini, A., Pomi, R., Rossi, A., Sarasini, F., Tirillò, J., & Zonfa, T. (2023). Anaerobic biodegradation of disposable PLA-based products: assessing the correlation with physical, chemical and microstructural properties. Journal of Hazardous Materials, 452, 131244. https://doi.org/10.1016/j.jhazmat.2023.131244. PMid:36965354. 50. Davarcioglu, B., & Rashidi, A. (2017). Characterization of clayey soils and physical properties of their compressed earth blocks from Central Anatolia: a case study. Journal of Multidisciplinary Engineering Science and Technology, 4(8), 7932-7942. Retrieved in 2025, August 10, from http://jmest. org/wp-content/uploads/JMESTN42352351.pdf 51. Bednarz, P., Bernasik, A., & Laska, J. (2018). The influence of sterilization on properties of polyurethane/polylactide blend. Science. Technology and Innovation, 2(1), 13-18. https://doi. org/10.5604/01.3001.0012.1264. 52. Bodirlau, R., Spiridon, I., & Teaca, C. A. (2007). Chemical investigation of wood tree species in a temperate forest eastnorthern Romania. BioResources, 2(1), 41-57. https://doi. org/10.15376/biores.2.1.41-57. 53. Villaquirán-Caicedo, M. A., Perea, V. N., Ruiz, J. E., & de Gutiérrez, R. M. (2021). Mechanical, physical and thermoacoustic properties of lightweight composite geopolymers. Ingeniería y Competitividad, 24(1). https://doi.org/10.25100/iyc. v24i1.10985. 54. Yuniarto, K., Purwanto, Y. A., Purwanto, S., Welt, B. A., Purwadaria, H. K., & Sunarti, T. C. (2016). Infrared and Raman studies on polylactide acid and polyethylene glycol-400 blend. AIP Conference Proceedings, 1725(1), 020101. https://doi. org/10.1063/1.4945555. 55. Bouamer, A., Benrekaa, N., Younes, A., & Amar, H. (2018). Characterization of the Polylactic acid stretched uniaxial and annealed by Raman spectrometry and Differential scanning calorimetry. IOP Conference Series. Materials Science and Engineering, 461, 012006. https://doi.org/10.1088/1757899X/461/1/012006. 56. Xu, H., Yang, X., Xie, L., & Hakkarainen, M. (2016). Conformational Footprint in Hydrolysis-Induced Nanofibrillation and Crystallization of Poly(lactic acid). Biomacromolecules, 17(3), 985-995. https://doi.org/10.1021/acs.biomac.5b01636. PMid:26820906. 57. Krasowska, K., & Heimowska, A. (2023). Degradability of polylactide in natural aqueous environments. Water, 15(1), 198. https://doi.org/10.3390/w15010198. 58. Haryńska, A., Janik, H., Sienkiewicz, M., Mikolaszek, B., & Kucińska-Lipka, J. (2021). PLA-potato thermoplastic starch filament as a sustainable alternative to the conventional pla filament: processing, characterization, and FFF 3D printing. ACS Sustainable Chemistry & Engineering, 9(20), 6923-6938. https://doi.org/10.1021/acssuschemeng.0c09413. 59. Ambrosio, G., Faglia, G., Tagliabue, S., & Baratto, C. (2021). Study of the Degradation of Biobased Plastic after Stress Tests in Water. Coatings, 11(11), 1330. https://doi.org/10.3390/ coatings11111330. 9/11
Boechat, L. N. F., Amorim, R. G., Reis, F. S., Pinto, M. O. C. M., Bispo, E. R., Middea, A., Lima, E. M. B., Bigansolli, A. R., Carmo, D. M., Lima-Kühn, B. B., Azevedo Meleiro, C. H., Castro, R. N., & Oliveira, R. N. 60. Tripathi, N., Misra, M., & Mohanty, A. K. (2021). Durable polylactic acid (PLA)-based sustainable engineered blends and biocomposites: recent developments, challenges, and opportunities. ACS Engineering Au, 1(1), 7-38. https://doi. org/10.1021/acsengineeringau.1c00011. 61. Limsukon, W., Rubino, M., Rabnawaz, M., Lim, L.-T., & Auras, R. (2023). Hydrolytic degradation of poly(lactic acid): unraveling correlations between temperature and the three phase structures. Polymer Degradation & Stability, 217, 110537. https://doi.org/10.1016/j.polymdegradstab.2023.110537. 62. Giełdowska, M., Puchalski, M., Sztajnowski, S., & Krucińska, I. (2022). Evolution of the molecular and supramolecular structures of PLA during the thermally supported hydrolytic degradation of wet spinning fibers. Macromolecules, 55(22), 10100-10112. https://doi.org/10.1021/acs.macromol.2c01778. 63. Janczak, K., Dąbrowska, G. B., Raszkowska-Kaczor, A., Kaczor, D., Hrynkiewicz, K., & Richert, A. (2020). Biodegradation of the plastics PLA and PET in cultivated soil with the participation of microorganisms and plants. International Biodeterioration & Biodegradation, 155, 105087. https://doi.org/10.1016/j. ibiod.2020.105087. 64. Jeong, S. B., Heo, K. J., & Lee, B. U. (2019). Antimicrobial air filters using natural sea salt particles for deactivating airborne bacterial particles. International Journal of Environmental Research and Public Health, 17(1), 190. https://doi.org/10.3390/ ijerph17010190. PMid:31892112.
10/11
65. Satti, S. M., Shah, A. A., Marsh, T. L., & Auras, R. (2018). Biodegradation of poly(lactic acid) in soil microcosms at ambient temperature: evaluation of natural attenuation, bio-augmentation and bio-stimulation. Journal of Polymers and the Environment, 26(9), 3848-3857. https://doi.org/10.1007/ s10924-018-1264-x. 66. Daneluz, J., Favero, J. S., Santos, V., Weiss-Angeli, V., Gomes, L. B., Mexias, A. S., & Bergmann, C. P. (2020). The influence of different concentrations of a natural clay material as active principle in cosmetic formulations. Materials Research, 23(2), e20190572. https://doi.org/10.1590/1980-5373-mr-2019-0572. 67. Erkul, S. N., & Ucaroglu, S. (2025). The effect of applying treatment sludge and vermicompost to soil on the biodegradability of poly(lactic acid) and poly(3-hydroxybutyrate). Polymers, 17(3), 352. https://doi.org/10.3390/polym17030352. PMid:39940554. 68. Vieira, A. C., Vieira, J. C., Guedes, R. M., & Marques, A. T. (2010). Degradation and viscoelastic properties of PLA-PCL, PGA-PCL, PDO and PGA Fibres. Materials Science Forum, 636-637, 825-832. https://doi.org/10.4028/www.scientific.net/ MSF.636-637.825. Received: Aug. 10, 2025 Revised: Mar. 02, 2026 Accepted: Mar. 16, 2026 Associate Editor: César L. Petzhold
Polímeros, 36(2), e20260023, 2026
Polylactic acid with oat oil: a biodegradable material intended for food packaging
Supplementary Material Supplementary material accompanies this paper. Table S1. FTIR vibrational modes of PLA and PLA-OO (oat oil) samples. “ν” means “stretching”; “δ” represents “deformation” or “bending”; “ρ” means “rocking”; “s” is “symmetrical”. Table S2. Samples’ Raman peaks. PLA is the main component in all samples, so only the peaks that do not correspond to PLA in PLA-oat oil samples were pointed out as oat oil ones. “ν” means “stretching”; “δ” represents “deformation” or “bending”; “τ” is “twisting”; “ρ” means “rocking”; “s” is “symmetrical”; and “as” is “asymmetrical”. Table S3. I_875⁄I_1452 values of original and degraded samples in two media (seawater and soil). Figure S1. (a) FTIR and (b) Raman spectra, as well as (c) XRD diffractogram of PLA; PLA-5OO, PLA-10OO, and PLA-15OO samples, zoomed is the crystallite size (D) results; (d) is the samples’ mechanical (maximum) strength. Figure S2. Samples’ degradation in (a) seawater and (b) soil. Figure S3. Polynomial fit of degradation regarding PLA-5OO, PLA-10OO, and PLA-15OO in both media, (a-c) seawater and (d-f) soil, respectively. Figure S4. FTIR analysis of degraded and non-degraded samples: (a) PLA, (b) PLA-5OO, (c) PLA-10OO, (d) PLA-15OO. Figure S5. Raman analysis of degraded and non-degraded samples: (a) PLA, (b) PLA-5OO, (c) PLA-10OO, (d) PLA-15OO. Figure S6. XRD diffractograms of the samples degraded in seawater and soil: (a) PLA, (b) PLA-5OO, (c) PLA-10OO, (d) PLA-15OO. Figure S7. Mechanical properties (tensile at break strength) of the samples. This material is available as part of the online article from https://doi.org/10.1590/0104-1428.20250073
Polímeros, 36(2), e20260023, 2026
11/11
ISSN 1678-5169 (Online)
https://doi.org/10.1590/0104-1428.20250116
Ferula biomass: characterization and biosorption studies for the removal of dyes Moubarek Mébarki1* , Hassiba Bokhari2 , Yasmina Benabdesslem1 , Ahmed Khelifaoui3 & Kadda Hachem2,4 Department of Agronomy And Nutrition Sciences, Faculty of Nature and Life Sciences, University of Saida Dr. Moulay Tahar, BP 138 ENNASR, 20000 Saida, Algeria 2 Plant and Microbial Production and Valorization Laboratory - LP2VM, Faculty of Nature and Life Sciences, University of Science and Technology of Oran Mohamed Boudiaf, Oran, Algeria 3 Laboratory of Chemistry, Synthesis, Properties and Applications, Department of Chemistry, Faculty of Technology, University of Saida - Dr. Moulay Tahar, Saida, Algeria 4 Higher Normal School of Saida, Saida, Algeria 1
*mebarek.mebarki@univ-saida.dz
Abstract The manufacture and industrial use of dyes generate highly colored, often non-biodegradable effluents that pose serious environmental and public health risks.The aim of this study was to evaluate the capacity of ferula stems from the Saida region to serve as a biosorbent in the treatment of water synthetically contaminated with two dyes, Congo Red (CR) and Methylene Blue (MB). The results of XRD, FTIR, SEM, and EDS analyses confirm that ferula stems biomass has an amorphous lignocellulosic structure with functional groups and surface characteristics that favor dye adsorption. MB shows a higher adsorption capacity than CR, with a maximum retention of 33.83 mg/g versus 21.0 mg/g for CR. In competitive adsorption, the biomass showed a greater affinity for MB with 85% at higher concentrations. Adsorption data were well described by the Langmuir isotherm (R2 ≈ 0.95). These results demonstrate the promising applicability of Ferula biomass for treating dye-contaminated waters. Keywords: biosorption, methylene blue, Congo red, Ferula communis biomass. Data Availability: All data supporting the findings of this study are included in this article. How to cite: Mébarki, M., Bokhari, H., Benabdesslem, Y., Khelifaoui, A., & Hachem, K. (2026). Ferula biomass: characterization and biosorption studies for the removal of dyes. Polímeros: Ciência e Tecnologia, 36(2), e20260024. https://doi.org/10.1590/0104-1428.20250116
1. Introduction Water pollution affecting rivers, seas, water tables, and lakes, whether accidentally or deliberately, by certain chemicals of industrial (hydrocarbons, phenols, dyes, etc.) or agricultural (pesticides, fertilizers, etc.) origin is a source of ecosystem degradation[1]. The problem is even more serious in the case of industrial effluents, which are much more toxic[2,3]. Organic dyes are widely used in a variety of industries, including dyeing leather, paper, textiles, wood, silk, and plastics, as well as in the cosmetics, food, and pharmaceutical sectors[4]. Among these, methylene blue and congo red are among the most commonly used dyes for dyeing various materials, such as silk, cotton and wood, as well as for the temporary dyeing of paper. These dyes also serve as colored indicators in redox reactions, histological stains, and antiseptics for the treatment of superficial wounds[5,6]. However, many studies have shown that these dyes can have harmful health effects[7], such as a faster heart rate, problems with the reproductive system[8], and trouble breathing[9].The chromophore structure of dye molecules, which contains
Polímeros, 36(2), e20260024, 2026
aromatic rings and azo groups, likely contributes to these adverse effects. It is therefore crucial to develop sustainable and effective strategies to reduce the environmental risks associated with these substances[10]. Available techniques for removing organic dyes from water include photocatalytic degradation[11], ion exchange[12], catalytic redox[13], precipitation[14], and adsorption[13,15]. Among these methods, adsorption stands out as an economical and promising solution, thanks to its many advantages, such as low cost, low energy consumption, high separation efficiency, and ease of use[16]. Recently, extensive research has focused on the use of plant-based biomass and agricultural residues as low-cost, renewable, and environmentally friendly biosorbents for dye removal[17,18]. Many natural biosorbents, such as acorns pericarps[19], date stones[20], peanut shells[10], and Algerian carob shells[21], have been utilized as adsorbents for removing pollutants such as dyes and heavy metal ions. Efficient adsorption of methylene blue using various plant-derived biomasses has
1/13
O O O O O O O O O O O O O O O O
Mébarki, M., Bokhari, H., Benabdesslem, Y., Khelifaoui, A., & Hachem, K. been reported by Deniz and Tezel Ersanli[22], Dabagh et al.[23], and Choudhry et al.[24], while effective removal of Congo red using natural and modified biosorbents has been demonstrated by Fakhar et al.[25], Zubair et al.[26], and Manzoor et al.[27]. These studies highlight the crucial role of surface functional groups and pore structure in enhancing adsorption performance. Despite these advances, most reported biosorbents are derived from a limited number of plant sources, and the exploration of new, regionally abundant biomass remains insufficient. In particular, fast-growing perennial plants native to semi-arid regions have received little attention as potential dye adsorbents, highlighting a clear research gap. In Algeria, common Ferula biomass (Ferula communis L.), represents an interesting option as a fast-growing perennial plant that reaches 2 to 3 meters in height. Its thick, smooth, branched stems contain exploitable biomass.To the best of our knowledge, no previous study has reported the use of Ferula communis stem biomass for the adsorption of synthetic dyes such as methylene blue and congo red. Therefore, the novelty of this study lies in the first-time investigation of Ferula communis stems as a low-cost, natural biosorbent for the simultaneous removal of an anionic dye (Congo red) and a cationic dye (methylene blue) from aqueous solutions. The main objectives of this work are to: (i) characterize the physicochemical properties of Ferula communis stem biomass, (ii) evaluate its adsorption performance toward MB and CR under different experimental conditions, (iii) investigate the adsorption kinetics, isotherms, and thermodynamic behavior, and (iv) assess its potential as a sustainable alternative to conventional adsorbents for wastewater treatment.
2. Materials and Methods 2.1 Plant material The samples used in this study are Ferula communis stems. Harvesting took place in September 2023 in the old Saïda forest, located at coordinates 34°48’45.5 “N 0°09’43.5 ”E. After cleaning, the stems were manually detached and air-dried at ambient temperature (25 ± 2°C) for 72 h, followed by oven drying at 40°C for an additional 24 h to ensure complete moisture removal. Stems were pulverized to a particle size of less than 200 µm. The samples were then placed in a desiccator at room temperature.
2.2 Characterization X-ray diffraction (XRD) analysis of Ferula biomass was done using a Bruker D8 Advance diffractometer with a LynxEye fast detector and Cu Kα radiation (λ = 0.15432 nm). Approximately 1 g of biomass samples was prepared in powder form for analysis. Measurements were carried out using a Cu X-ray source (40 kV, 40 mA, 2.2 kW). Angular scanning was performed in the 2θ range from 5° to 120°, with a scanning speed of 2°/min. For data collection between 0.5° and 5°, a regular scan mode was used. Ferula biomass was analyzed using Fourier Transform Infrared Spectroscopy (FTIR) and Scanning Electron Microscopy with Energy Dispersive X-ray Spectroscopy (SEM/EDX). Biomass samples were pressed into pellets 2/13
using ATR mode both before and after dye adsorption to find out which functional groups were involved in the process. FTIR spectra were recorded using an Agilent Technologies Cary 600 spectrophotometer within the 400–4000 cm−1 range. Surface morphology and elemental composition were analyzed using a JEOL JSM-6610 SEM operating at an accelerating voltage of 20 kV, with magnifications ranging from ×250 to ×10,000, using a secondary electron detector. EDX analysis (EX-9430054L1Q, JEOL) was conducted on the biosorbents before and after dye adsorption, confirming dye fixation on the Ferula biomass surface.
2.3 Biosorption process All chemicals and reagents used in this study were of analytical grade. Methylene blue (MB, purity ≥ 99%) and Congo red (CR, purity ≥ 98%) dyes were purchased from Sigma-Aldrich and used without further purification. Stock solutions (1000 mg/L) of MB and CR were prepared by dissolving accurately weighed amounts of each dye in distilled water and stored in amber glass bottles at room temperature. Working solutions of desired concentrations (20–70 mg/L) were freshly prepared by appropriate dilution of the stock solutions. Adsorption experiments were carried out by bringing 0.1 g of Ferula biomass into contact with 50 mL of dye solution. The tests were carried out in a shaker at 280 rpm, centrifuged for 2 min at 5,000 rpm and then analyzed. The initial concentrations used were 20, 30, 40, 50, 60, and 70 mg/L. Samples were taken after an equilibration time of 2 hours. To study the selectivity of Ferula biomass, we tested its retention capacity in the presence of both dyes at identical initial concentrations of 20, 30, 40, 50, 60, and 70 mg/L, with a stable mass of 0.1 g at pH 5. We then shook them for 120 min. at 280 rpm. The quantity of dye (MB or CR) adsorbed per gram of biomass, qe (mg/g), is calculated according to the following formula:
qe =
( Ci − Ce )V
(1)
m
where Ci and Ce are, respectively, the initial and final dye concentrations in solution, expressed in mg/L. V is the volume of the solution in liters, and M is the mass of Ferula biomass in grams. The unadsorbed dye concentration was measured using a UV-Vis spectrophotometer. A 1 mL sample of the solution was taken, and its absorbance was measured by spectrophotometry at 498 nm for CR and 664 nm for MB.
3. Results and Discussions 3.1 Characterization 3.1.1 X-ray diffraction (XRD) analyses The diffractogram of Ferula biomass (Figure 1) shows a main peak at 2θ ≈ 22°, which is typical for cellulose, indicating that there is some crystalline structure like what is found in lignocellulosic fibers [28]. A second, wider peak seen at 2θ ≈ 22° indicates that there are some disordered or partly ordered areas, which are likely due to hemicellulose and lignin [29]. Polímeros, 36(2), e20260024, 2026
Ferula biomass: characterization and biosorption studies for the removal of dyes The overall profile indicates that the biomass has a predominantly amorphous structure, with locally crystallized zones. This XRD pattern is consistent with those reported for other plant-based biosorbents such as date pits, banana peel, sawdust, and carob shell, which also exhibit a combination of amorphous lignin-rich phases and crystalline cellulose domains [30,31]. The predominance of the amorphous phase is advantageous for adsorption processes, as it increases the accessibility of surface functional groups and enhances dye–biomass interactions[27,32] . Similar diffraction features were reported for biomass used in MB and CR adsorption, respectively[33,34]. 3.1.2 FTIR characterization The FTIR spectrum of Ferula biomass before it absorbs dye shows a peak at 656 cm−1, which is linked to the bending of C–OH groups, and a peak at 825 cm−1 that relates to C–H changes in cellulose. A band at 1072 cm−1 shows C–O stretching in polysaccharides[35]. The signal at 1389 cm−1 is related to C–H bending in polysaccharides and Caryl–O movements in syringyl units[36]. Peaks at 1507 cm−1 and
1595 cm−1 are related to the vibrations of the structure in lignin, and the band around 1647 cm−1 shows the stretching of C=O in carboxylates. The absorption at 2891 cm−1 comes from the stretching of C–H bonds and vibrations of CH2, while the wide band at 3318 cm−1 shows the presence of hydrogen-bonded O–H groups in cellulose and lignin. These functional groups (–OH, –COOH, –C=O, and aromatic rings) are widely recognized as active adsorption sites in lignocellulosic biosorbents, facilitating electrostatic attraction, hydrogen bonding, and π–π interactions with dye molecules[37]. Similar FTIR signatures have been reported for various biomass materials used for MB and CR removal, including peanut shells, rice husk, and fruit peels[38,39]. After dye adsorption (Figure 2), noticeable shifts and intensity changes were observed in the bands associated with O–H (≈3318 cm−1), C=O (≈1647 cm−1), and aromatic C=C (≈1507–1595 cm−1), confirming their direct involvement in the biosorption process. These spectral changes are consistent with the formation of surface complexes and non-covalent interactions between dye molecules and biomass functional groups, as reported in similar adsorption studies[29,32,37].
Figure 1. XRD diagram of Ferula biomass.
Figure 2. FTIR spectra of Ferula biomass (FB) before and after methylene blue (MB) and/or Congo red (RC) biosorption. Polímeros, 36(2), e20260024, 2026
3/13
Mébarki, M., Bokhari, H., Benabdesslem, Y., Khelifaoui, A., & Hachem, K. 3.1.3 SEM and EDS SEM micrographs and EDS spectra of Ferula biomass before and after dye biosorption are shown in Figures 3, 4, and 5. The Ferula biomass has an amorphous structure with no distinct surface morphology. Such surface roughness and porosity are favorable for adsorption, as they increase the surface area and provide more active sites for dye uptake[40,41]. Comparable surface features have been reported for other biosorbents derived from agricultural residues, such as coconut shell, walnut shell, and corn cob[27,36,42]. After biosorption, the surface becomes rough and irregular, suggesting dye adsorption in the form of aggregates. This morphological change after adsorption is a common indicator of successful dye fixation and has been observed in previous studies involving MB and CR adsorption onto plant-based biosorbents[27,43].
EDS spectra of pristine biomass reveal Ca, C and O peaks, reflecting the presence of O-H and -COOH functional groups, without detection of dyes. After exposure to the dyes, Ca peaks diminish and characteristic methylene blue and Congo red signals appear, confirming their adsorption to the biosorbent. Similar EDS trends have been reported in studies on dye adsorption using lignocellulosic and mineral-modified biosorbents[38,44] .
3.2 Biosorption 3.2.1 Effect of initial dye concentrations The biosorption of MB and CR was studied on a biomass fraction (Ferula comminus) as a function of the initial concentration of the MB and CR solution (20-70 mg/L). For each dye, the apparent ultimate adsorption capacity (qe) and percentage adsorption (% removal) were calculated. The results are shown in Table 1 and Figure 6.
Figure 3. (a) SEM and (b) EDS of Ferula biomass. 4/13
Polímeros, 36(2), e20260024, 2026
Ferula biomass: characterization and biosorption studies for the removal of dyes The graphs shown in the figure and the data summarized in the table indicate a decrease in the removal rate of MB (from 94.5% to 83.7%) and CR (from 82.7% to 55.2%) as the initial concentrations of MB and CR solutions increase. On the other hand, the amount of dye adsorbed (qe) increased from 9.45 to 29.30 mg/g for BM and from
8.27 to 19.32 mg/g for CR. The amount of adsorption (qe) increases with increasing concentration for both MB or CR. This phenomenon can be explained by the increase in the concentration gradient as the initial concentration rises, thus increasing the diffusion of dye molecules in solution at the adsorbent surface[45].
Figure 4. (a) SEM and (b) EDS of Ferula biomass after biosorption of methylene blue
Table 1. Results obtained with initial concentrations of MB and CR on Ferula biomass Ci (mg/L) Ce (mg/L) qe (mg/g) %removal
20 1.11 9.45 94.5
30 2.51 13.74 91.6
Ce (mg/L) qe (mg/g) %removal
3.45 8.27 82.7
6.69 11.66 77.7
Polímeros, 36(2), e20260024, 2026
Methylene Blue 40 3.41 18.30 91.5 Congo Red 9.98 15.01 75.1
50 4.88 22.56 90.2
60 9.48 25.26 84.2
70 11.40 29.30 83.7
21.27 14.37 57.5
24.37 17.82 59.4
31.35 19.32 55.2
5/13
Mébarki, M., Bokhari, H., Benabdesslem, Y., Khelifaoui, A., & Hachem, K.
Figure 5. (a) SEM and (b) EDS of Ferula biomass after biosorption of Congo Red.
Figure 6. Percentage elimination as a function of initial Methylene blue and Congo red concentrations (pH = 5 ; m = 0.1 g; V = 50 mL). 6/13
Polímeros, 36(2), e20260024, 2026
Ferula biomass: characterization and biosorption studies for the removal of dyes 3.2.2 Effect of initial solution pH The effect of initial pH on MB and CR adsorption was evaluated at Ci = 20 mg/L, m = 0.1 g, and V = 50 mL. The results are presented in Table 2 and Figure 7. Adsorption is clearly pH-dependent, as pH controls both the surface charge/protonation state of biomass functional groups and the ionization/speciation of dye molecules. For MB (cationic), the highest removal efficiency (89.13%) was observed at pH 6, indicating that moderately acidic to near-neutral conditions favor electrostatic attraction and hydrogen bonding with oxygen-containing functional groups (–OH, –COOH, C=O). In contrast, CR (anionic) exhibited minimum removal at pH 6 (44.73%) and improved adsorption under alkaline conditions (pH 8–10, ≈66%), suggesting that electrostatic interactions, hydrogen bonding, and possible dye aggregation jointly influence adsorption behavior. This trend is consistent with previous studies on pH-dependent adsorption of cationic and anionic dyes onto lignocellulosic biosorbents [34,38]
The thermodynamic parameters were calculated using K = qe/Ce and the van’t Hoff equation. The results are presented in Table 4. The thermodynamic parameters, calculated from van’t Hoff plot, are: ΔH° ≈ +1.65 kJ/mol; ΔS° ≈ −5.28 J/(mol•K) for MB; and ΔH° ≈ −12.26 kJ/mol; ΔS° ≈ −54.29 J/(mol•K) for CR adsorption.
3.2.3 Effect of contact time The effect of contact time on dye adsorption was investigated at Ci = 20 mg/L, m = 0.1 g, and V = 50 mL. The results are presented in Table 3 and Figure 8. Adsorption is rapid and approaches equilibrium within 90–120 min, which is characteristic of biosorption processes on porous lignocellulosic materials. The initial fast uptake is attributed to abundant available surface sites and external mass transfer, followed by a slower stage governed by intraparticle diffusion and site saturation. For MB, high removal (~95%) is achieved within 30 min, while CR adsorption increases more gradually, reaching ~92.65% at 120 min, indicating a slightly longer equilibration time. Minor non-monotonic variations (e.g., MB at 120 min) can be attributed to experimental scatter, sampling effects, or minor desorption phenomena, and are commonly reported in adsorption studies[20,23,45].
Figure 7. Effect of initial solution pH on the removal efficiency of methylene blue (MB) and Congo red (CR) by Ferula biomass (Ci = 20 mg/L; m = 0.1 g; V = 50 mL).
3.2.4 Effect of temperature and thermodynamic parameters The effect of temperature on MB and CR adsorption was evaluated at pH 6, contact time = 1 h, and Ci = 20 mg/L.
Figure 8. Effect of contact time on the removal efficiency of MB and CR (Ci = 20 mg/L; m = 0.1 g; V = 50 mL).
Table 2. Effect of initial pH on MB and CR adsorption by Ferula biomass (Ci = 20 mg/L; m = 0.1 g; V = 50 mL). pH 2 4 6 8 10
MB Ce (mg/L) 2.65 3.49 2.17 4.16 3.29
MB qe (mg/g) 8.67 8.25 8.91 7.91 8.35
MB Removal (%) 86.70 82.51 89.13 79.15 83.50
CR Ce (mg/L) 7.15 8.39 11.05 6.80 6.80
CR qe (mg/g) 6.42 5.80 4.47 6.60 6.60
CR Removal (%) 64.27 58.07 44.73 66.02 66.02
Table 3. Effect of contact time on MB and CR adsorption (Ci = 20 mg/L; m = 0.1 g; V = 50 mL). Time (min) 30 60 90 120 150
MB Ce (mg/L) 1.04 0.91 0.72 1.11 0.72
Polímeros, 36(2), e20260024, 2026
MB qt (mg/g) 9.48 9.55 9.64 9.45 9.64
MB Removal (%) 94.80 95.45 96.40 94.45 96.40
CR Ce (mg/L) 2.78 2.91 2.30 1.47 1.47
CR qt (mg/g) 8.61 8.55 8.85 9.27 9.27
CR Removal (%) 86.10 85.45 88.50 92.65 92.65
7/13
Mébarki, M., Bokhari, H., Benabdesslem, Y., Khelifaoui, A., & Hachem, K. For CR, the negative ΔH° value indicates an exothermic adsorption process, consistent with the observed decrease in qe and increase in Ce with rising temperature. The negative ΔS° values suggest decreased randomness at the solid–liquid interface due to dye molecule ordering on the biomass surface. The positive ΔG° values reflect K < 1 under the studied conditions, indicating a non-spontaneous trend at the tested concentration and contact time. However, this result should be interpreted cautiously, as robust thermodynamic evaluation typically requires equilibrium constants derived from complete isotherm datasets at multiple temperatures, as recommended in adsorption thermodynamics studies[8,25,40,41]. Positive ΔG° values result from using K = qe/Ce, which is not a true equilibrium constant; therefore, ΔG° does not reflect spontaneity accurately. Proper thermodynamic analysis requires dimensionless K from multitemperature isotherms.
Figure 9 shows the variation in removal efficiency as a function of the initial concentration of both MB and CR. Analysis of the Figure 9 shows an increase in MB removal efficiency at higher initial concentrations, with removal rates exceeding 85%. The removal efficiency of CR is very low compared with MB, which does not exceed 60% at concentrations of Ci =60 mg/L. This may be due to the chemical nature of each dye, since MB is a positively charged cationic dye that favors their interaction on biomass chemical groups such as the hydroxyl functions of cellulose and the carboxyl functions of pectin [46]. Also this difference can be explained by several mechanistic factors, including electrostatic interactions, molecular size, and steric effects. Electrostatically, MB is a cationic dye, which promotes strong attraction toward negatively charged functional groups on the biomass surface, such as hydroxyl (–OH) groups of cellulose and carboxyl (–COOH) groups of pectin [29]. In contrast, CR is an anionic dye and therefore experiences electrostatic repulsion with negatively charged surface sites, reducing its adsorption efficiency. In addition, molecular size and structure play a key role. CR has a larger molecular size and a more complex,
3.2.5 Competitiveness results In this parameter we mixed two dyes, methylene blue and congo red to examine the effect of the competitiveness of the two dyes on the adsorption capacity of Ferula communis biomass. The adsorption data obtained are shown in Table 5.
Figure 9. The effect of MB+CR competitiveness on Ferula biomass (pH = 5; m = 0.1 g; V = 50 mL).
Table 4. Thermodynamic dataset and Gibbs free energy changes for MB and CR adsorption. T (K) MB Ce (mg/L) MB qe (mg/g) KMB (=qe/Ce) ΔG°MB (kJ/mol) CR Ce (mg/L) CR qe (mg/g) KCR (=qe/Ce) ΔG°CR (kJ/mol) 298 12.65 3.675 0.2905 +3.063 14.15 2.925 0.2067 +3.906 318 13.49 3.255 0.2413 +3.759 15.39 2.305 0.1498 +5.020 333 12.17 3.915 0.3217 +3.140 16.05 1.975 0.1231 +5.801
Table 5. Representation of the effect of the competitiveness of the two dyes (MB+CR) on Ferula biomass
8/13
Ci (mg/L) Ce (mg/L) qe (mg/g) %removal
20 4.29 7.85 78.5
30 6.74 11.63 77.5
Ce (mg/L) qe (mg/g) %removal
14.95 2.52 25.2
16.61 6.69 44.6
MB 40 7.72 16.14 80.7 CR 23.26 8.37 41.9
50 7.16 21.42 85.7
60 11.06 24.27 81.6
70 10.36 29.82 85.2
22.92 13.54 45.2
23.42 18.29 61.0
31.10 19.45 55.6
Polímeros, 36(2), e20260024, 2026
Ferula biomass: characterization and biosorption studies for the removal of dyes elongated azo structure compared to MB, which hinders its diffusion into the pores of the biomass and limits access to active adsorption sites. This steric hindrance further reduces its uptake relative to MB. 3.2.6 Isotherm modeling: The different models used in this study are the Langmuir model and the Freundlich model. The following observations can be made from the Table 6 data: The maximum adsorption capacity for MB (33.89 mg/g) and for CR (21.00 mg/g). The R2 correlation coefficients are between 0.97 and 0.95 for both models, underlining the good repeatability of the experimental results[19]. The Langmuir isotherm modeling of the experimental results is exploited in the linear form (1/qe vs. 1/Ce) is shown in Figure 8. The Langmuir model shows an excellent degree of linearization with R2 between 0.95 and 0.97. Furthermore, the (KL= 0.011) is high for CR compared to MB with (KL= 0.002). The fraction tested has a (qmax) of 33.89 mg/g for MB and 21.00 mg/g for CR. These results exceed the values recently reported by several studies on Methylene Blue and Congo Red (Table 7). The plot of log (qe) versus log (Ce) for the adsorption of methylene blue and Congo red on the Ferula biomass is shown in Figure 8. A high KF indicates a high adsorption capacity. Methylene blue showed a KF = 2.64 mg/g, while Congo red showed a KF = 2.16 mg/g. 1/n estimates adsorption intensity or surface heterogeneity. A value of 1/n close to zero indicates adsorbent heterogeneity[51]. Methylene blue with 0.47 is more heterogeneous than Congo red with 0.33. The adsorption capacity of MB is more favorable than that of CR with 0.47 and 0.33 respectively.
From the results obtained, we can see that the correlation coefficient values obtained from Langmuir modeling are excellent compared to Freundlich modeling. We can therefore say that the Langmuir model better describes the biosorption kinetics of MB and CR than the Freundlich model. The Temkin and Dubinin–Radushkevich (D–R) shown in Figure 10 results provide complementary insight into the surface–adsorbate interaction energetics for MB and CR on Ferula communis biomass. The Temkin model assumes that the heat of adsorption decreases linearly with surface coverage (i.e., adsorbent–adsorbate interactions and energetic heterogeneity are considered), and the good Temkin correlations obtained—particularly for MB (R2 ≈ 0.97) and reasonably for CR (R2 ≈ 0.89)—suggest that adsorption occurs on an energetically nonuniform surface where interaction strength changes progressively as sites are occupied[52]. In Temkin, the constants A (related to binding affinity) and B (related to adsorption heat/interaction term) indicate that MB shows a higher interaction term (B ≈ 8.39 mg/g) than CR (B ≈ 4.43 mg/g), consistent with a stronger overall interaction of MB with the biomass functional groups under test conditions[40,53]. The D–R model, based on the Polanyi potential, is often used to estimate the mean adsorption energy (E) and infer whether the uptake is predominantly physical adsorption (typically E < 8 kJ/mol) rather than stronger chemisorption/ionexchange regimes. The calculated E values for both dyes are well below 8 kJ/mol (MB ≈ 1.11 kJ/mol; CR ≈ 0.52 kJ/mol), supporting that physisorption dominates (e.g., van der Waals forces, π–π interactions, and hydrogen bonding) even though other models (e.g., PSO kinetics) may also fit well due to surfacesite availability effects[53].
Table 6. Langmuir, Freundlich, Temkin and Dubinin–Radushkevich (D–R) isotherm parameters for MB and CR adsorption onto Ferula communis biomass. Colorants MB CR MB CR
qmax(mg/g) 33.89 21.00 Temkin A (L/g) 2.551 2.079
Langmuir KL(L/mg) 0.002 0.011 Temkin B (mg/g) 8.390 4.427
R2 0.97 0.95 R2 0.967 0.885
KF [(mg/g) (L/mg/)1/n] 2.64 2.16 D–R qm (mg/g) 24.09 16.77
Freundlich 1/n 0.47 0.33 D–R β (mol2/J2) 4.04 × 10−7 1.88 × 10−6
R2 0.96 0.88 D–R E (kJ/mol) 1.113 0.515
Table 7. Comparison of our results (qmax) for Ferrula biomass with values recently reported by several works on the two dyes (MB and CR). Adsorbents Ferula stem Carob shells Date stones Neem leaf powder Chamomile bark Chir pine Activated carbon Trichoderma.Virens Trichoderma.Viride
Polímeros, 36(2), e20260024, 2026
Colorants MB CR MB MB MB CR CR CR CR CR
qmax (mg/g) 33.89 21.0 13.17 23.8 41.5 25.84 5.8 10.68 5.57 2.70
References Our results [21] [47] [48] [40] [49] [50]
9/13
Mébarki, M., Bokhari, H., Benabdesslem, Y., Khelifaoui, A., & Hachem, K. Finally, the moderate D–R fits (R2 ≈ 0.83–0.86) indicate that D–R captures part of the adsorption energetics but does not fully describe all heterogeneity/interaction effects, so it is best interpreted together with Temkin and Langmuir/ Freundlich as recommended in isothermmodel selection guidelines. 3.2.7 Kinetic modeling To better understand the adsorption mechanism and rate-controlling steps, the experimental kinetic data for methylene blue (MB) and Congo red (CR) adsorption onto Ferula biomass were fitted to three widely used kinetic models: the pseudo-first-order (PFO), pseudo-second-order (PSO), and intraparticle diffusion (IPD) models[54]. The linearized forms of these models are given as follows: Pseudo-first-order ( PFO ) : ln ( qe − qt )=
ln ( qe ) − k1t
(2)
Pseudo-second-order ( PSO = ) :t / qt 1/ k 2qe2 + t / qe (3)
Intraparticle diffusion ( IPD = ) : qt
kid t1/ 2 + C
(4)
where qt(mg/g) is the adsorption capacity at time t (min), qe (mg/g) is the equilibrium adsorption capacity, k1 (1/min) and k2 (g/mg/min) are the rate constants of the PFO and PSO models, respectively, kid (mg·g−1·min−1/2) is the intraparticle diffusion rate constant, and C (mg/g) is the intercept related to boundary-layer thickness (film diffusion contribution)[40]. The kinetic parameters obtained from linear regression analysis are summarized in Table 8. For both MB and CR, the PSO model provided the best fit, with correlation coefficients (R2> 0.99) and calculated equilibrium adsorption capacities (qe,calc) closely matching the experimental values (qe). This indicates that chemisorption involving valence forces through electron sharing or exchange between dye molecules and surface functional groups is likely the dominant rate-controlling mechanism, as widely reported for dye adsorption onto lignocellulosic biosorbents[8,40,45,46]. The PFO model showed lower correlation coefficients and poorer agreement between calculated and experimental qe values, suggesting that it does not adequately describe the adsorption kinetics of MB and CR on Ferula biomass.
Figure 10. Linearized isotherm plots for methylene blue (MB) and congo red (CR) adsorption on Ferula communis biomass: (a) Langmuir (1/qe vs 1/Ce), (b) Freundlich (log qe vs log Ce), (c) Temkin (qe vs ln Ce), and (d) Dubinin–Radushkevich (ln qe vs ε2).
Table 8. Kinetic parameters for MB and CR adsorption onto Ferula biomass (Ci = 20 mg/L; m = 0.1 g; V = 50 mL).
10/13
Dye
Model
qe (mg/g)
qe calc (mg/g)
Rate constant
R2
MB MB MB CR CR CR
PFO PSO IPD PFO PSO IPD
9.64 9.64 – 9.27 9.27 –
8.97 9.71 – 8.61 9.34 –
k1 = 0.031 1/min k2 = 0.014 g/mg/min kid = 0.74 mg·g−1·min−1/2, C = 3.12 mg/g k1 = 0.024 1/min k2 = 0.010 g/mg/min kid = 0.68 mg·g−1·min−1/2, C = 3.85 mg/g
0.942 0.996 0.918 0.934 0.993 0.905
Polímeros, 36(2), e20260024, 2026
Ferula biomass: characterization and biosorption studies for the removal of dyes The IPD plots did not pass through the origin, as reflected by the non-zero intercept (C), indicating that intraparticle diffusion is involved in the adsorption process but is not the sole rate-limiting step. This suggests that adsorption occurs via multiple stages, including external mass transfer, surface adsorption, and intraparticle diffusion, consistent with observations reported for other plant-based biosorbents[27,37,42]. Recent studies further support the adsorption behaviors observed in this work. Research on dyebiosorbent systems has shown that surface functional groups and surface charge play a decisive role in enhancing adsorption performance, particularly for ionic dyes, where electrostatic interactions dominate uptake mechanisms. Likewise, recent analyses of competitive adsorption highlight that adsorbents often demonstrate preferential binding toward cationic species, consistent with the stronger affinity of our Ferula biomass for MB compared to CR.[55-58].
• Funding acquisition – Moubarek Mébarki; Hassiba Bokhari; Kadda Hachem. • Investigation – Moubarek Mébarki; Yasmina Benabdesslem; Kadda Hachem. • Methodology – Moubarek Mébarki; Kadda Hachem. • Project administration – NA. • Resources – Moubarek Mébarki; Ahmed Khelifaoui. • Software – NA. • Supervision –Yasmina Benabdesslem; Kadda Hachem. • Validation – Hassiba Bokhari; Yasmina Benabdesslem; Kadda Hachem. • Visualization –Yasmina Benabdesslem. • Writing – original draft – Moubarek Mébarki. • Writing – review & editing – Moubarek Mébarki; Hassiba Bokhari.
4. Conclusions
6. Acknowledgments
This study evaluated the effectiveness of Ferula communis stem biomass as a lowcost biosorbent for the removal of methylene blue (MB) and congo red (CR) dyes from aqueous solutions. According to the analysis, it was found that: Characterization techniques reveal that Ferrule biomass has a predominantly amorphous structure with areas of crystallized cellulose and functional groups (C=O, O-H, C-H) involved in biosorption. Changes in surface morphology and elemental analysis after adsorption confirm effective dye fixation, validating its potential as a biosorbent. Of the two dyes we used, MB absorbed better. MB dye exhibited maximum retention capacity on Ferula biomass, reaching 33.89 mg/g versus 21.0 mg/g for CR. The biomass preferentially adsorbs Methylene Blue over Congo Red due to favorable electrostatic interactions, highlighting its selectivity towards cationic dyes. All these results show that the Langmuir model is relevant for describing biosorption mechanisms. With regard to future prospects, further work is planned with the aim of: Explore the biosorption of Ferula stem biomass with a wider range of dyes, as well as other organic pollutants such as pesticides, phenols, and heavy metals. Examine other parameters likely to influence adsorption capacity, and real wastewater testing. In conclusion, the use of Ferula stem biomass is emerging as a new approach for decontaminating dyepolluted waters. This use looks promising for the future of wastewater purification. It is conceivable that the use of biomass residues could be more advantageous than traditional physicochemical treatment methods.
We thank Sara. Khlef and Nabila. Miloudi from the University of Saida - Dr. Moulay Tahar, for their contribution in Batch biosorption experiments.
5. Author’s Contribution • Conceptualization – Moubarek Mébarki; Hassiba Bokhari; Ahmed Khelifaoui; Yasmina Benabdesslem; Kadda Hachem. • Data curation – Moubarek Mébarki; Yasmina Benabdesslem; Kadda Hachem. • Formal analysis – Moubarek Mébarki; Hassiba Bokhari; Ahmed Khelifaoui. Polímeros, 36(2), e20260024, 2026
7. References 1. Barka, N., Abdennouri, M., El Makhfouk, M., & Qourzal, S. (2013). Biosorption characteristics of cadmium and lead onto eco-friendly dried cactus (opuntia ficus indica) cladodes. Journal of Environmental Chemical Engineering, 1(3), 144-149. https://doi.org/10.1016/j.jece.2013.04.008. 2. Anyaene, I. H., Onukwuli, O. D., Babayemi, A. K., ObioraOkafo, I. A., & Ezeh, E. M. (2023). Application of Bio coagulation–flocculation and soft computing aids for the removal of organic pollutants in aquaculture effluent discharge. Chemistry Africa, 7(1), 455-478. https://doi.org/10.1007/ s42250-023-00754-9. 3. Arica, T. A., Ayas, E., & Arica, M. Y. (2017). Magnetic mcm41 silica particles grafted with poly(glycidylmethacrylate) brush: modification and application for removal of direct dyes. Microporous and Mesoporous Materials, 243, 164-175. https://doi.org/10.1016/j.micromeso.2017.02.011. 4. Robati, D., Mirza, B., Rajabi, M., Moradi, O., Tyagi, I., Agarwal, S., & Gupta, V. K. (2016). Removal of hazardous dyes-br 12 and methyl orange using graphene oxide as an adsorbent from aqueous phase. Chemical Engineering Journal, 284, 687-697. https://doi.org/10.1016/j.cej.2015.08.131. 5. Sakr, F., Sennaoui, A., Elouardi, M., Tamimi, M., & Assabbane, A. (2015). Étude de l’adsorption du bleu de méthylène sur un biomatériau à base de cactus (adsorption study of methylene blue on biomaterial using cactus). Journal of Materials & Environmental Sciences, 6(2), 397-406. Retrieved in 2025, December 20, from https://www.jmaterenvironsci.com/ Document/vol6/vol6_N2/48-JMES-1115-2014-Sakr.pdf 6. Arica, T. A., Kuman, M., Gercel, O., & Ayas, E. (2019). Poly(dopamine) grafted bio-silica composite with tetraethylenepentamine ligands for enhanced adsorption of pollutants. Chemical Engineering Research & Design, 141, 317-327. https://doi.org/10.1016/j.cherd.2018.11.003. 7. Maimaiti, T., Hu, R., Yuan, H., Liang, C., Liu, F., Li, Q., Lan, S., Yu, B., & Yang, S.-T. (2022). Magnetic Fe3O4/ TiO2/graphene sponge for the adsorption of methylene blue in aqueous solution. Diamond and Related Materials, 123, 108811. https://doi.org/10.1016/j.diamond.2021.108811. 11/13
Mébarki, M., Bokhari, H., Benabdesslem, Y., Khelifaoui, A., & Hachem, K. 8. Mouni, L., Belkhiri, L., Bollinger, J.-C., Bouzaza, A., Assadi, A., Tirri, A., Dahmoune, F., Madani, K., & Remini, H. (2018). Removal of methylene blue from aqueous solutions by adsorption on kaolin: kinetic and equilibrium studies. Applied Clay Science, 153, 38-45. https://doi.org/10.1016/j.clay.2017.11.034. 9. Tohdee, K., Kaewsichan, L., & Asadullah, (2018). Enhancement of adsorption efficiency of heavy metal Cu(ii) and Zn(ii) onto cationic surfactant modified bentonite. Journal of Environmental Chemical Engineering, 6(2), 2821-2828. https://doi.org/10.1016/j. jece.2018.04.030. 10. Reghioua, A., Atia, D., Hamidi, A., Jawad, A. H., Abdulhameed, A. S., & Mbuvi, H. M. (2024). Production of eco-friendly adsorbent of kaolin clay and cellulose extracted from peanut shells for removal of methylene blue and congo red removal dyes. International Journal of Biological Macromolecules, 263(Pt 1), 130304. https:// doi.org/10.1016/j.ijbiomac.2024.130304. PMid:38382796. 11. Wang, S. (2019). Algal and alginate based beads and foams as sorbents for metal sorption and catalyst supports for 3-nitrophenol hydrogenation (Doctoral dissertation). Université de Montpellier, Montpellier, France. https://doi.org/10.70675 /734149c7z8d93z492az8fe6z610d2d175457 12. Abdel-Aziz, M. H., Nirdosh, I., & Sedahmed, G. H. (2013). Ion-exchange-assisted electrochemical removal of heavy metals from dilute solutions in a stirred-tank electrochemical reactor: a mass-transfer study. Industrial & Engineering Chemistry Research, 52(33), 11655-11662. https://doi.org/10.1021/ ie400548w. 13. Ajenifuja, E., Ajao, J. A., & Ajayi, E. O. B. (2017). Adsorption isotherm studies of Cu (ii) and Co (ii) in high concentration aqueous solutions on photocatalytically modified diatomaceous ceramic adsorbents. Applied Water Science, 7(7), 3793-3801. https://doi.org/10.1007/s13201-017-0527-3. 14. Agwaramgbo, L., Magee, N., Nunez, S., & Mitt, K. (2013). Biosorption and chemical precipitation of lead using biomaterials, molecular sieves, and chlorides, carbonates, and sulfates of na & ca. Journal of Environmental Protection, 4(11), 1251-1257. https://doi.org/10.4236/jep.2013.411145. 15. Bayramoglu, G., Acikgoz-Erkaya, I., Celikbicak, O., & Arica, M. Y. (2026). Use of free and entrapped spirogyra sp. algae to remove endocrine-disrupting chemicals from polluted waters through biological intervention. Water, Air, and Soil Pollution, 237(9), 514. https://doi.org/10.1007/s11270-026-09207-8. 16. Afroze, S., & Sen, T. K. (2018). A review on heavy metal ions and dye adsorption from water by agricultural solid waste adsorbents. Water, Air, and Soil Pollution, 229(7), 225. https:// doi.org/10.1007/s11270-018-3869-z. 17. Kassa, A., Engida, A., & Endaye, M. (2025). Eco-friendly adsorbents for industrial dye removal: a comprehensive review of low-cost alternatives. Desalination and Water Treatment, 323, 101362. https://doi.org/10.1016/j.dwt.2025.101362. 18. Khan, T. A., Nazir, M., & Khan, E. A. (2013). Adsorptive removal of rhodamine b from textile wastewater using water chestnut (trapa natans l.) peel: adsorption dynamics and kinetic studies. Toxicological and Environmental Chemistry, 95(6), 919-931. https://doi.org/10.1080/02772248.2013.840369. 19. Mébarki, M., Hachem, K., Gloaguen, V., & Faugeron-Girard, C. (2022). Removal of metallic cations from aqueous solutions using acorn pericarp fractions of quercus ilex as new biosorbents. International Journal of Environmental Science and Technology, 20(4), 3613-3620. https://doi.org/10.1007/s13762-022-04253-1. 20. Khelifi, O., Mehrez, I., Ben Salah, W., Ben Salah, F., Younsi, M., Nacef, M., & Affoune, A. M. (2016). Study of methylene blue (MB) adsorption from aqueous solutions on biosorbent prepared from Algerian date stones. LARHYSS Journal, 28, 135-148. Retrieved in 2025, December 20, from http://www. larhyss.net/ojs/index.php/larhyss/article/view/464/456 12/13
21. Bensafiddine, F., Benalia, M., Hadj Seyd, A., Djedid, M., Ad, C., Baba Amar, Z., & Elmsellem, H. (2020). Biosorption of heavy metals (Copper, Nickel) and dye (Methylene Bleu) from aqueous solution onto southern Algerian carob shells. Moroccan Journal of Chemistry, 8(3), 638-646. https://doi. org/10.48317/IMIST.PRSM/morjchem-v8i3.21217. 22. Deniz, F., & Tezel Ersanli, E. (2022). A novel biowaste-based biosorbent material for effective purification of methylene blue from water environment. International Journal of Phytoremediation, 24(12), 1243-1250. https://doi.org/10.1080/ 15226514.2021.2025039. PMid:35014910. 23. Dabagh, A., Ait Ichou, A., Benhiti, R., Abali, M., EL-Habacha, M., Sinan, F., & Zerbet, M. (2024). Removal of methylene blue from aqueous solutions by adsorption onto carpobrotus edulis biomass. Bioremediation Journal, 1-16. https://doi.org/ 10.1080/10889868.2024.2382266. 24. Choudhry, A., Sharma, A., Siddiqui, S. I., Ahamad, I., Sajid, M., Khan, T. A., & Chaudhry, S. A. (2023). Origanum vulgare manganese ferrite nanocomposite: an advanced multifunctional hybrid material for dye remediation. Environmental Research, 220, 115193. https://doi.org/10.1016/j.envres.2022.115193. PMid:36587717. 25. Fakhar, N., Khan, S. A., Khan, T. A., & Siddiqi, W. A. (2022). Efficiency of iron modified pyrus pyrifolia peels biochar as a novel adsorbent for methylene blue dye abatement from aqueous phase: equilibrium and kinetic studies. International Journal of Phytoremediation, 24(11), 1173-1183. https://doi. org/10.1080/15226514.2021.2021848. PMid:34990566. 26. Zubair, M., Manzar, M. S., Khan, S. A., Suleiman, M. A., Nawaz, M., Khan, T. A., Bakather, O. Y., Gama, B. M. V., Yasir, M., Melli, L., & Khan, G. (2025). Enhanced adsorption of anionic dyes onto naoh modified green coffee waste biochar: characteristics and performance evaluation. International Journal of Environmental Science and Technology, 22(9), 7721-7738. https://doi.org/10.1007/s13762-024-06090-w. 27. Manzoor, K., Batool, M., Naz, F., Nazar, M. F., Hameed, B. H., & Zafar, M. N. (2024). A comprehensive review on application of plant-based bioadsorbents for congo red removal. Biomass Conversion and Biorefinery, 14(4), 4511-4537. https://doi. org/10.1007/s13399-022-02741-5. 28. Alfattani, R., Shah, M. A., Siddiqui, M. I. H., Ali, M. A., & Alnaser, I. A. (2022). Bio-char characterization produced from walnut shell biomass through slow pyrolysis: sustainable for soil amendment and an alternate bio-fuel. Energies, 15(1), 1. https://doi.org/10.3390/en15010001. 29. Vassilev, S. V., Baxter, D., Andersen, L. K., Vassileva, C. G., & Morgan, T. J. (2012). An overview of the organic and inorganic phase composition of biomass. Fuel, 94, 1-33. https://doi.org/10.1016/j.fuel.2011.09.030. 30. Bhatnagar, A., & Sillanpää, M. (2010). Utilization of agroindustrial and municipal waste materials as potential adsorbents for water treatment: a review. Chemical Engineering Journal, 157(2-3), 277-296. https://doi.org/10.1016/j.cej.2010.01.007. 31. Crini, G. (2006). Non-conventional low-cost adsorbents for dye removal: a review. Bioresource Technology, 97(9), 1061-1085. https://doi.org/10.1016/j.biortech.2005.05.001. PMid:15993052. 32. Long, Z., Wang, Z., Huang, Q., Jia, Y., Jiao, Z., Wang, Y., & Du, Y. (2024). High-performance adsorption of methylene blue using novel bio-adsorbent based on sargassum fusiforme. Heliyon, 10(18), e37949. https://doi.org/10.1016/j.heliyon.2024. e37949. PMid:39381252. 33. Kayan, G. Ö., & Kayan, A. (2021). Composite of natural polymers and their adsorbent properties on the dyes and heavy metal ions. Journal of Polymers and the Environment, 29(11), 3477-3496. https://doi.org/10.1007/s10924-021-02154-x. Polímeros, 36(2), e20260024, 2026
Ferula biomass: characterization and biosorption studies for the removal of dyes 34. Stjepanović, M., Velić, N., Galić, A., Kosović, I., Jakovljević, T., & Habuda-Stanić, M. (2021). From waste to biosorbent: removal of congo red from water by waste wood biomass. Water (Basel), 13(3), 279. https://doi.org/10.3390/w13030279. 35. Faix, O. (1992). Fourier transform infrared spectroscopy. In S. Y. Lin & C. W. Dence (Eds.), Methods in lignin chemistry (pp. 233-241). USA: Springer. https://doi.org/10.1007/978-3-642-74065-7_16 36. Collier, W. E., Schultz, T. P., & Kalasinsky, V. F. (1992). Infrared study of lignin: reexamination of aryl-alkyl ether c—o stretching peak assignments. Holzforschung - International Journal of the Biology, Chemistry. Holzforschung, 46(6), 523-528. https://doi.org/10.1515/hfsg.1992.46.6.523. 37. Kumar, A., Singh, R., Upadhyay, S. K., Kumar, S., & Charaya, M. U. (2021). Biosorption: the removal of toxic dyes from industrial effluent using phytobiomass-a review. Plant Archives, 21(Suppl 1), 1320-1325. https://doi.org/10.51470/ PLANTARCHIVES.2021.v21.S1.207. 38. Sawalha, H., Bader, A., Sarsour, J., Al-Jabari, M., & Rene, E. R. (2022). Removal of dye (methylene blue) from wastewater using bio-char derived from agricultural residues in palestine: performance and isotherm analysis. Processes (Basel, Switzerland), 10(10), 2039. https://doi.org/10.3390/pr10102039. 39. Ungureanu, E. L., Mocanu, A. L., Stroe, C. A., Panciu, C. M., Berca, L., Sionel, R. M., & Mustatea, G. (2023). Agricultural byproducts used as low-cost adsorbents for removal of potentially toxic elements from wastewater: a comprehensive review. Sustainability (Basel), 15(7), 5999. https://doi.org/10.3390/ su15075999. 40. Sathya, K., Jayalakshmi, H., Reddy, S. N., Ratnam, M. V., & Bandhu, D. (2023). Effective removal of congo red dye using adsorbent prepared from bio-waste: isotherm, kinetic, and thermodynamic studies. Biomass Conversion and Biorefinery, 15(3), 3557-3569. https://doi.org/10.1007/s13399-023-05213-6. 41. Khan, T. A., Rahman, R., & Khan, E. A. (2016). Decolorization of bismarck brown R and crystal violet in liquid phase using modified pea peels: non-linear isotherm and kinetics modeling. Modeling Earth Systems and Environment, 2(3), 141. https:// doi.org/10.1007/s40808-016-0195-6. 42. Kali, A., Amar, A., Loulidi, I., Jabri, M., Hadey, C., Lgaz, H., Alrashdi, A. A., & Boukhlifi, F. (2024). Characterization and adsorption capacity of four low-cost adsorbents based on coconut, almond, walnut, and peanut shells for copper removal. Biomass Conversion and Biorefinery, 14(3), 3655-3666. https:// doi.org/10.1007/s13399-022-02564-4. 43. Kaur, N., Kaushal, J., Mahajan, P., & Mantri, A. (2024). Phytoremediation of methylene blue dye (triarylmethane) and congo red (diazo) by T. ammi L.: kinetic studies. International Journal of Environmental Science and Technology, 21(2), 1697-1714. https://doi.org/10.1007/s13762-023-05037-x. 44. Namasivayam, C., & Kavitha, D. (2006). IR, xrd and sem studies on the mechanism of adsorption of dyes and phenols by coir pith carbon from aqueous phase. Microchemical Journal : Devoted to the Application of Microtechniques in All Branches of Science, 82(1), 43-48. https://doi.org/10.1016/j. microc.2005.07.002. 45. Li, H., Budarin, V. L., Clark, J. H., North, M., & Wu, X. (2022). Rapid and efficient adsorption of methylene blue dye from aqueous solution by hierarchically porous, activated starbons®: mechanism and porosity dependence. Journal of Hazardous Materials, 436, 129174. https://doi.org/10.1016/j. jhazmat.2022.129174. PMid:35739710. 46. Padhi, D. K., Parida, K. M., & Singh, S. K. (2016). Mechanistic aspects of enhanced congo red adsorption over graphene oxide in presence of methylene blue. Journal of Environmental Chemical Engineering, 4(3), 3498-3511. https://doi.org/10.1016/j. jece.2016.07.011.
Polímeros, 36(2), e20260024, 2026
47. Mulugeta, M., & Lelisa, B. (2014). Removal of methylene blue (MB) dye from aqueous solution by bioadsorption onto untreated parthenium hystrophorous weed. Modern Chemistry & Applications, 2(4), 1000146. https://doi.org/10.4172/2329-6798.1000146. 48. Hassan, M. A. (2025). Neem leaf powder an economical adsorbent for methylene blue removal. Results in Surfaces and Interfaces, 21, 100646. https://doi.org/10.1016/j.rsurfi.2025.100646. 49. Khan, T. A., Sharma, S., Khan, E. A., & Mukhlif, A. A. (2014). Removal of congo red and basic violet 1 by chir pine (Pinus roxburghii) sawdust, a saw mill waste: batch and column studies. Toxicological and Environmental Chemistry, 96(4), 555-568. https://doi.org/10.1080/02772248.2014.959017. 50. Argumedo-Delira, R., Gómez-Martínez, M. J., & UribeKaffure, R. (2021). Trichoderma biomass as an alternative for removal of congo red and malachite green industrial dyes. Applied Sciences (Basel, Switzerland), 11(1), 448. https://doi. org/10.3390/app11010448. 51. Haroon, H., Gardazi, S. M. H., Butt, T. A., Pervez, A., Mahmood, Q., & Bilal, M. (2017). Novel lignocellulosic wastes for comparative adsorption of Cr(VI): equilibrium kinetics and thermodynamic studies. Polish Journal of Chemical Technology, 19(2), 6-15. https://doi.org/10.1515/pjct-2017-0021. 52. Khan, T. A., Nazir, M., & Khan, E. A. (2016). Magnetically modified multiwalled carbon nanotubes for the adsorption of bismarck brown r and Cd (II) from aqueous solution: batch and column studies. Desalination and Water Treatment, 57(41), 19374-19390. https://doi.org/10.1080/19443994.2015.1100553. 53. Mechnou, I., Meskini, S., Elqars, E., Chham, A.-I., & Hlaibi, M. (2024). Classical and advanced isotherms to model the adsorption of drugs, dyes and metals on activated carbonaceous materials: a review. Environmental Chemistry Letters, 22(5), 2375-2404. https://doi.org/10.1007/s10311-024-01759-7. 54. Hussain, D., Khan, S. A., Alharthi, S. S., & Khan, T. A. (2022). Insight into the performance of novel kaolinite-cellulose/cobalt oxide nanocomposite as green adsorbent for liquid phase abatement of heavy metal ions: modelling and mechanism. Arabian Journal of Chemistry, 15(7), 103925. https://doi. org/10.1016/j.arabjc.2022.103925. 55. Shelke, B. N., Jopale, M. K., & Kategaonkar, A. H. (2022). Exploration of biomass waste as low cost adsorbents for removal of methylene blue dye: a review. Journal of the Indian Chemical Society, 99(7), 100530. https://doi.org/10.1016/j. jics.2022.100530. 56. Shelke, B. N., Jopale, M. K., Chavan, K. U., Gaware, M. R., & Kategaonkar, A. H. (2024). Biosorption of methylene blue by lentil shell on activation with sulfuric acid, formaldehyde, and calcination: kinetic, isotherm, and thermodynamic study. Journal of Dispersion Science and Technology, 45(10), 19091919. https://doi.org/10.1080/01932691.2023.2234989. 57. Shelke, B. N., Jopale, M. K., Pratap, U. R., & Kategaonkar, A. H. (2024). Optimization of orange g and indigo carmine dye sequestration by incense stick ash: characterisation, isotherm, and kinetic analysis. Biomass Conversion and Biorefinery, 14(20), 25251-25262. https://doi.org/10.1007/s13399-023-04579-x. 58. Badawi, A. K., Abd Elkodous, M., & Ali, G. A. (2021). Recent advances in dye and metal ion removal using efficient adsorbents and novel nano-based materials: an overview. RSC Advances, 11(58), 36528-36553. https://doi.org/10.1039/D1RA06892J. PMid:35494372. Received: Dec. 20, 2025 Revised: Mar. 15, 2026 Accepted: Mar. 18, 2026 Editor-in-Chief: Sebastião V. Canevarolo
13/13
ISSN 1678-5169 (Online)
https://doi.org/10.1590/0104-1428.20250079
S Development of a glycerol–CuSO4 polymer for high gamma S ionizing radiation dosimetry S Gabriela Pontes Cardoso , Jony Marques Geraldo and Adriana de Souza Medeiros Batista * S Departamento de Engenharia Nuclear, Universidade Federal de Minas Gerais – UFMG, Belo Horizonte, MG, Brasil S Departamento de Anatomia e Imagem, Universidade Federal de Minas Gerais – UFMG, Belo Horizonte, MG, Brasil S Hospital Luxemburgo, Belo Horizonte, MG, Brasil Hospital Alberto Cavalcanti, Fundação Hospitalar do Estado de Minas Gerais, Belo Horizonte, MG, Brasil S S Abstract This study presents a novel glycerol-based polymeric material doped with 0.12% (w/w) copper (II) sulfate pentahydrate S for high-dose gamma dosimetry. Upon irradiation with doses ranging from 10 to 250 kGy using a Cobalt-60 source, the initially greenish material exhibited a progressive color change from yellow to dark red. Two analytical approaches were employed to evaluate the dosimetric potential: UV-Vis spectrophotometry, which demonstrated an exponential increase S in absorbance at 456 nm up to 70 kGy, and digital image analysis using ImageJ, which extended the useful dose range to 250 kGy through measurements of green channel optical measurements. Both methods yielded reproducible calibration curves, highlighting the material’s potential as a low-cost, easy-to-handle dosimeter. This short communication reports S preliminary findings that support further investigation into the material’s dosimetric mechanisms and optimization. S Keywords: copper sulfate pentahydrate, gamma dosimetry, glycerol-based polymer, ImageJ analysis, UV-Vis spectrophotometry. Data Availability: All data supporting the findings of this study are available from the corresponding author upon request. S How to cite: Cardoso, G. P., Geraldo, J. M., & Batista, A. S. M. (2026). Development of a glycerol–CuSO polymer for S high gamma ionizing radiation dosimetry. Polímeros: Ciência e Tecnologia, 36(2), e20260017. https://doi.org/10.1590/01041428.20250079. S 1. Introduction S Radiation dosimetry plays a crucial role in ensuring the investigated: (i) optical density analysis via scanned images safety and efficacy of processes involving ionizing radiation, processed with ImageJ software, and (ii) ultraviolet-visible S particularly in industrial and medical applications. Among the (UV-Vis) spectrophotometry. various dosimetric systems developed, polymer-based materials S have gained attention due to their versatility, low cost, and ease of processing. Colorimetric dosimeters, in particular, 2. Materials and Methods offer a simple and visual means of dose estimation, often S A single formulation was prepared for this study, relying on radiation-induced chemical changes that result in 1
2,3,4
1,2
1
2
3
4
*adriananuclear@yahoo.com.br
4
measurable optical variations[1]. Glycerol-based polymeric matrices have been explored for various applications due to their biocompatibility, transparency, and ability to incorporate additives[2]. The incorporation of metal salts into such matrices can lead to functional materials with tunable optical and chemical properties. Copper (II) sulfate pentahydrate (CuSO4·5H2O), a well-known inorganic compound, exhibits distinct colorimetric behavior and has been studied in different polymeric systems[1,3]. However, its potential role in radiation dosimetry, particularly in inducing color changes upon gamma irradiation, remains underexplored. In this context, we report the development of a novel glycerol-based material doped with 0.12% (w/w) copper (II) sulfate pentahydrate, which exhibits a distinct color change upon exposure to high doses of gamma radiation. Two dosimetric approaches were
Polímeros, 36(2), e20260017, 2026
consisting of a glycerol-based polymeric matrix doped with copper (II) sulfate pentahydrate. The base composition included 100 mL of bidistilled glycerin (Farmax®), 100 mL of clinical ultrasound gel (Mercur®), 24 g of unflavored gelatin, and 1.5 mL of formaldehyde solution. In the test formulation, 0.3 g of copper (II) sulfate pentahydrate (CuSO4·5H2O, molar mass: 249.68 g/mol, Synth®) was previously dissolved in the ultrasound gel before mixing with the other components. This corresponds to an approximate concentration of 0.12% (w/w) or 0.15% (w/v) in the final formulation. During preparation, the liquid formulation was poured into a rectangular mold (25 × 15 cm) where it gelled, forming a firm, greenish structure about 2 mm thick. It was cut into 2 × 2 cm pieces, stored in high-density polyethylene bags, and analyzed by ultraviolet-visible
1/4
Cardoso, G. P., Geraldo, J. M., & Batista, A. S. M. (UV-Vis) spectrophotometry and ImageJ software under the same dimensions without any change in thickness or size. The samples were irradiated with gamma radiation at doses of 10 and 250 kGy, using a constant dose rate. The irradiation process was conducted in the multipurpose irradiator of the Gamma Irradiation Laboratory (LIG), located at the Center for the Development of Nuclear Technology (CDTN), and equipped with a Cobalt-60 source. Dosimetric characterization was performed using two complementary approaches. The first approach employed ultraviolet-visible (UV-Vis) spectrophotometry, conducted using a Kasvi® spectrophotometer, with readings acquired in the wavelength range of 300 to 900 nm. Absorbance values were used to generate exponential dose-response curves, reinforcing the
material’s potential for high-dose gamma dosimetry. The second approach involved digital image analysis of the irradiated samples using the ImageJ software. The images were acquired using an HP Deskjet Plus Ink Advantage 6476 scanner, and optical density values were extracted from the green channel of RGB (Red, Green, Blue) images. These values were used to construct exponential calibration curves correlating optical response with absorbed dose.
3. Results and Discussions Figure 1 presents the results obtained from ultravioletvisible (UV-Vis) spectrophotometry and visual inspection of the samples subjected to gamma irradiation. The absorption
Figure 1. UV-Vis absorption spectra of irradiated samples (a), exponential calibration curve based on absorbance at 456 nm (b), and visual color variation of samples as a function of gamma dose (c). The photographic panel includes intermediate doses for illustrative purposes, even though only selected doses were used to construct the calibration curve shown in (b). 2/4
Polímeros, 36(2), e20260017, 2026
Development of a glycerol–CuSO4 polymer for high gamma ionizing radiation dosimetry spectra, recorded between 300 and 900 nm, exhibited two prominent features: a sharp peak at approximately 456 nm and a broader band centered around 715 nm. As the absorbed dose increased, the absorbance at 456 nm progressively intensified, while the signal at 715 nm decreased. This opposing behavior suggests the occurrence of radiationinduced chemical transformations within the material. The absorption band observed near 715 nm in the non-irradiated samples is consistent with d–d transitions of hydrated Cu (II) ions, as similarly reported for Cu–CMD (carboxymethyl dextran) complexes at 744 nm[4]. The progressive decrease of this band with increasing gamma dose suggests radiation-induced chemical transformations, possibly involving dehydration or oxidation of Cu (II) species, supporting the hypothesis of partial conversion to copper oxide. The spectral evolution suggests that gamma irradiation may be attributed to the formation of copper oxide species, as reported for CuO nanoparticles in the literature, although this was not confirmed in this study[5]. However, this interpretation is hypothetical and based on previous studies; no direct evidence of nanoparticle formation was obtained in this work. To quantify the dosimetric response, a calibration curve was constructed by plotting the absorbance at 456 nm against the irradiation dose. The resulting curve followed an exponential trend, described by Equation 1, indicating a nonlinear but predictable increase in absorbance with dose. The exponential behavior aligns with typical polymeric systems where radiation induces progressive chromophoric transformations. = y y0 + Ae(
x/t )
(1)
where y is the absorbance measured at 456 nm; x is the absorbed gamma dose (in kGy); y0 is the baseline absorbance (i.e., the
absorbance when the dose is zero); A is the amplitude of the absorbance change induced by irradiation; t is the exponential constant related to the material’s sensitivity to radiation. Although the material was irradiated across a wide range (10 to 250 kGy), the most reliable and sensitive response was observed up to 70 kGy, defining the practical dosimetric range for this system. Complementing the spectroscopic data, a photographic panel of the samples illustrates the progressive color change induced by irradiation. The nonirradiated sample appears greenish-yellow, while samples exposed to increasing doses transition through yellow, brown, and ultimately dark red at 250 kGy. This visual progression aligns with the UV-Vis findings and reinforces the potential of the material as a colorimetric dosimeter. To complement the UV-Vis spectrophotometric analysis and extend the dosimetric evaluation within the useful range up to 70 kGy, digital image processing was employed using the ImageJ software. Optical density values were extracted from the green channel of RGB images of the irradiated samples, allowing quantification of the color change induced by gamma radiation (Figure 2). The resulting data were plotted as a function of the absorbed dose, and an exponential fit was applied to describe the dose-response behavior. The curve followed Equation 2: = y y0 + A1e (
− x − x0 ) / t1
(2)
where y is the optical density in the green channel; x is the absorbed dose (kGy); y0 is the baseline optical density, representing the value when the dose effect stabilizes; x0 is the dose offset, indicating the point at which the exponential decay begins; A1 is the amplitude of the optical density change induced by irradiation; t1 is the exponential decay constant,
Figure 2. Exponential calibration curve based on green channel optical density extracted from sample images using ImageJ, as a function of gamma dose (kGy). Polímeros, 36(2), e20260017, 2026
3/4
Cardoso, G. P., Geraldo, J. M., & Batista, A. S. M. related to the rate at which the green channel intensity decreases with dose. In the curve fitting the parameter x0 was fixed at 30 kGy to improve model stability, as the experimental data did not provide sufficient sensitivity to estimate this offset reliably. Consequently, its uncertainty is zero, while the other parameters were freely adjusted and present nonzero uncertainties derived from the fitting algorithm. The curve demonstrates a consistent decrease in green channel intensity with increasing dose, reflecting the visual transition from greenish to reddish tones observed in the samples. It is important to note that the exponential equations used to model the dose-response behavior in UV-Vis and ImageJ analyses differ due to the nature of the data and the direction of the optical change. In the UV-Vis analysis, absorbance at 456 nm increases with dose, reflecting the accumulation of radiation-induced chromophores, and in contrast, the ImageJ analysis focuses on the green channel intensity extracted from RGB images, which decreases as the sample darkens with increasing dose. This behavior is best described by an exponential decay function, incorporating a dose offset to account for the initial response threshold. These distinct mathematical models accurately represent the respective optical phenomena and support the complementary use of both techniques in high-dose gamma dosimetry. Similar approaches using copper-based compounds as dosimetric indicators have been reported in the literature, such as copper-doped potassium sulfate for optically stimulated luminescence and polymer systems incorporating copper oxide nanoparticles, both demonstrating promising dosimetric properties under ionizing radiation[1,6].
4. Conclusions The results confirm the potential of the glycerolbased polymeric material doped with copper (II) sulfate pentahydrate as a viable candidate for high-dose gamma dosimetry, combining low cost, ease of preparation, and a clear optical response. To advance the understanding of the radiation-induced mechanisms responsible for the observed color change, future studies should investigate the chemical transformations and structural modifications occurring within the material. These analyses may help elucidate the formation and oxidation states of copper species, the role of the polymeric matrix in stabilizing chromophores, and the kinetics of the radiation–material interaction. A deeper comprehension of these processes will support the refinement of the formulation and contribute to improving its sensitivity, stability, and reproducibility under varying irradiation conditions. Future work should include FTIR and Raman spectroscopy to elucidate structural changes and long-term stability studies to assess the temporal performance of the developed dosimeter.
5. Author’s Contribution • Conceptualization – Gabriela Pontes Cardoso; Jony Marques Geraldo; Adriana de Souza Medeiros Batista. • Data curation – Gabriela Pontes Cardoso; Adriana de Souza Medeiros Batista. 4/4
• Formal analysis – Gabriela Pontes Cardoso; Adriana de Souza Medeiros Batista. • Funding acquisition – Adriana de Souza Medeiros Batista. • Investigation – Gabriela Pontes Cardoso; Adriana de Souza Medeiros Batista. • Methodology – Gabriela Pontes Cardoso; Jony Marques Geraldo; Adriana de Souza Medeiros Batista. • Project administration – Adriana de Souza Medeiros Batista. • Resources – Gabriela Pontes Cardoso; Adriana de Souza Medeiros Batista. • Software – Gabriela Pontes Cardoso. • Supervision – Jony Marques Geraldo; Adriana de Souza Medeiros Batista. • Validation – Adriana de Souza Medeiros Batista. • Visualization – Gabriela Pontes Cardoso; Adriana de Souza Medeiros Batista. • Writing – original draft – Gabriela Pontes Cardoso; Adriana de Souza Medeiros Batista. • Writing – review & editing – Adriana de Souza Medeiros Batista.
6. References 1. Salman, M. D., Radzi, Y. M., Oglat, A. A., Kolaib, R. W., Idris, A. S. A., Alhassan, M., Alton, W. A., & Rahman, A. A. (2025). Enhancing the acoustic properties for a novel radiation dosimetry PMMAG by optimizing the stability of copper oxide nanoparticles. BioNanoScience, 15(2), 278. https://doi. org/10.1007/s12668-025-01900-y. 2. Goyal, S., Hernández, N. B., & Cochran, E. W. (2021). An update on the future prospects of glycerol polymers. Polymer International, 70(7), 911-917. https://doi.org/10.1002/pi.6209. 3. Udhayakumari, D. (2025). Recent advances in colorimetric and fluorescent chemosensors for Cu2+ Ions: trends, challenges, and future directions. Journal of Fluorescence, 35(10), 9395-9412. https://doi.org/10.1007/s10895-025-04253-7. PMid:40095404. 4. Glišić, S., Nikolić, G., Cakić, M., & Trutić, N. (2015). Spectroscopic study of copper (II) complexes with carboxymethyl dextran and dextran sulfate. Russian Journal of Physical Chemistry A. Focus on Chemistry, 89(7), 1254-1262. https://doi.org/10.1134/ S0036024415070122. 5. Rajesh, S., Geetha, A., Guganathan, L., Suthakaran, S., Anbuvannan, M., Pragadeswaran, S., Santhamoorthy, M., Kim, S. C., Batoo, K. M., Ijaz, M. F., Mohammad, M. R., & Palaniappan, S. K. (2024). Enhanced photocatalytic performance of CuO nanoparticles synthesized via surfactant assisted hydrothermal method. Applied Physics. A, Materials Science & Processing, 130(9), 661. https://doi.org/10.1007/ s00339-024-07850-8. 6. Majgier, R., & Okada, G. (2023). Optically stimulated luminescence characteristics and dosimetric properties of copper-doped potassium sulphate. Journal of Luminescence, 257, 119702. https://doi.org/10.1016/j.jlumin.2023.119702. Received: Sep. 09, 2025 Revised: Nov. 25, 2025 Accepted: Jan. 19, 2026 Editor-in-Chief: Sebastião V. Canevarolo Polímeros, 36(2), e20260017, 2026
São Paulo 994 St. São Carlos, SP, Brazil, 13560-340 Phone: +55 16 3374-3949 Email: abpol@abpol.org.br 2021
2026